Gypsum floor sound insulation mortar and preparation process thereof
Through the preparation process of sound insulation mortar on the gypsum floor, combined with desulfurization gypsum, polyethylene particles, vapor phase silica particles, sepiolite fibers and suppository fibers, the existing mortar has been solved, and the problem of poor sound insulation performance and high density is achieved. It has light weight, high adhesion and excellent sound insulation, and is suitable for energy conservation and emission reduction in modern buildings.
Patent Information
- Application Number
- CN202411119886.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
The mortar on existing building floors does not have sound insulation properties, is dense and prone to hollowing and cracking, and cannot effectively reduce the impact and friction noise of residential floors.
The preparation process of sound insulation mortar on the floor of gypsum floor includes desulfurization gypsum, polyethylene particles, vapor phase silica particles, sepiolite fibers, suppository fibers, retarders, cellulose ethers, glue powders and deionized water combinations. By adding epoxy resin emulsion and pretreated polyvinyl alcohol fibers, a lightweight, high adhesion and excellent sound insulation properties are formed.
It realizes gypsum mortar with low density and good adhesion, has significant sound insulation effect, avoids hollowing and cracking problems, and improves the mechanical properties and crack resistance of the mortar. It is suitable for laying floors of 10-80mm thick floors.
Smart Images

Figure BDA0004994744530000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sound insulation mortar, in particular to a gypsum floor sound insulation mortar and a preparation process thereof. Background Art
[0002] With the improvement of living standards, people pay more and more attention to the sound insulation performance of building materials, and are very disgusted with the noise caused by the impact and friction of the upper floor of the house, which not only affects the sleep of the residents on the lower floors, but also affects people's mood. However, the ordinary mortar used in building floors today does not have the performance of sound insulation mortar. The existing sound insulation mortar also has problems such as high density, unsatisfactory sound insulation effect, easy hollowing and cracking. Therefore, there is an urgent need for a mortar with low density, good adhesion, light weight and excellent sound insulation performance to meet people's needs for interior design.
[0003] Based on this situation, the present application discloses a gypsum floor sound insulation mortar and a preparation process thereof to solve this technical problem. Summary of the invention
[0004] The object of the present invention is to provide a gypsum floor sound insulation mortar and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A gypsum floor sound insulation mortar, the components of the sound insulation mortar comprising, by weight, 60-80 parts of desulfurized gypsum, 6-12 parts of polyethylene particles, 5-10 parts of fumed silica particles, 4-8 parts of sepiolite fibers, 4-10 parts of cork fibers, 0.2-0.45 parts of retarder, 0.2-0.5 parts of cellulose ether, 1.5-3 parts of rubber powder, 0.2-0.6 parts of thixotropic enzyme, and 40-45 parts of deionized water.
[0007] In the more optimized solution, the desulfurized gypsum semi-aqueous phase is 80-85%; the particle size of the polyethylene particles is 2.5-3 mm, and the density is 50-60 kg / m 3 ; The particle size of the fumed silica particles is 1.8-2.5 mm, and the density is 40-50 kg / m 3 The sepiolite fiber has a length of 6 to 8 mm, a width of 0.8 to 1 mm, and a density of 250 to 300 kg / m 3 The length of cork fiber is 2-3 mm, the width is 0.5-0.8 mm, and the density is 160-180 kg / m 3 .
[0008] In a more optimized solution, the retarder is a protein-based gypsum retarder; the cellulose ether is hydroxypropyl methylcellulose ether with a viscosity of 100,000; the rubber powder is VAE rubber powder, and the thixotropic enzyme is a magnesium aluminum silicate lubricant.
[0009] According to a more optimized solution, the sound insulation mortar also includes epoxy resin emulsion and pretreated polyvinyl alcohol fiber, the amount of the epoxy resin emulsion accounts for 4-6wt% of the total mass of the desulfurized gypsum; the pretreated polyvinyl alcohol fiber accounts for 0.5-2.5wt% of the total mass of the desulfurized gypsum.
[0010] The most optimized scheme is that the preparation steps of the pretreated polyvinyl alcohol fiber are as follows: mixing concentrated nitric acid and deionized water, adding ammonium cerium nitrate, stirring evenly to obtain an ammonium cerium nitrate solution; mixing deionized water, polyvinyl alcohol fiber and glycidyl methacrylate, ultrasonically dispersing for 20 to 30 minutes to obtain a dispersion; adding 40 mL of the ammonium cerium nitrate solution to the dispersion, reacting at 40 to 45° C. for 5 to 6 hours, filtering and collecting the product, washing and drying to obtain the pretreated polyvinyl alcohol fiber;
[0011] The concentration of the concentrated nitric acid is 16 mol / L; the polyvinyl alcohol fiber is any one or more of trilobal polyvinyl alcohol fiber, quadrilobal polyvinyl alcohol fiber, triangular polyvinyl alcohol fiber and circular polyvinyl alcohol fiber.
[0012] According to a more optimized solution, the polyvinyl alcohol fiber is a compound of trilobal polyvinyl alcohol fiber and quadrilobal polyvinyl alcohol fiber, with a mass ratio of 2:3.
[0013] In a more optimized solution, the preparation steps of the epoxy resin emulsion are:
[0014] S1: Heat allyl glycidyl ether to 60-65°C, add chloroplatinic acid-isopropanol mixture, stir for 10-20 minutes, slowly drop 1,1,3,3-tetramethyldisiloxane, keep warm for 2-2.5 hours, cool and collect the product to obtain epoxysilane;
[0015] Mix epoxy silane and diethylenetriamine, raise the temperature to 70-75°C, and keep the temperature to react for 5-6 hours to obtain an amino-terminated curing agent;
[0016] S2: Mix the amino-terminated curing agent and diethylenetriamine, stir evenly to obtain a compound curing agent; mix the epoxy resin and the compound curing agent, stir for 20 to 30 minutes, and obtain an epoxy resin emulsion.
[0017] In a more optimized solution, in S1, the molar ratio of allyl glycidyl ether to 1,1,3,3-tetramethyldisiloxane is (2.1-2.4):1; the molar ratio of epoxysilane to diethylenetriamine is 1:(1.5-2);
[0018] In S2, the mass ratio of the amino-terminated curing agent to diethylenetriamine is (4-5):1; the mass ratio of the epoxy resin to the compound curing agent is (3-4):1.
[0019] A more optimized solution is a preparation process of a gypsum floor sound insulation mortar, and the specific steps are as follows:
[0020] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 to 2 minutes, and then adding the premix additive, stirring for 3 to 5 minutes to obtain a mixture;
[0021] Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
[0022] In a more optimized solution, step (2) is specifically as follows: mixing the epoxy resin emulsion and the pretreated polyvinyl alcohol fiber, stirring evenly to obtain a polymer solution; mixing the mixture, the polymer solution and deionized water, stirring evenly to obtain a sound insulation mortar.
[0023] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0024] This solution provides a mortar with low density, good adhesion, light weight and excellent sound insulation performance. And adjust its preparation process and formula. This solution uses desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fiber, cork fiber, retarder, cellulose ether, rubber powder and other components, mixed with deionized water to form gypsum mortar, in which no cement is added. The prepared gypsum mortar has excellent sound insulation effect and good adhesion. When practical, it can be used to lay 10-80mm thick floor slabs without hollowing or cracking, and has excellent performance.
[0025] The solution adds sepiolite fiber and uses the properties of sepiolite fiber to produce a damping structure to consume the noise generated by impact and friction, so that the mortar has a sound insulation function; at the same time, cork fiber itself has a sound-absorbing effect, and the reasonable combination with sepiolite fiber makes the mortar structure have a better anti-cracking and non-shrinkage effect than ordinary mortar. Polyethylene particles have the property of suspension in mortar, and will be evenly dispersed in the mortar body, attached to the mortar suspension, and will not settle when the mortar is laid to a certain thickness, which can effectively solve the problem of mortar bleeding, segregation, and sedimentation; combined with light materials such as fumed silica particles as aggregates, the volume is light, and the density of the sound insulation mortar is small, even more than twice that of traditional floor sound insulation mortar, and the weight is light, which can reduce the self-weight of high-rise buildings. It is an ideal material for energy conservation and emission reduction in modern buildings.
[0026] On this basis, this scheme also adds polyvinyl alcohol fiber and epoxy resin emulsion, and the polyvinyl alcohol fiber is any one or more of trilobal polyvinyl alcohol fiber, quadrilobal polyvinyl alcohol fiber, triangular polyvinyl alcohol fiber, and circular polyvinyl alcohol fiber. The optimal scheme is that the polyvinyl alcohol fiber is a compound of trilobal polyvinyl alcohol fiber and quadrilobal polyvinyl alcohol fiber, and the mass ratio is 2:3. The design of the special-shaped structure can enhance the interfacial properties of the polyvinyl alcohol fiber in the system. At the same time, the scheme carries out surface grafting modification on the polyvinyl alcohol fiber, introduces epoxy group, and mixes it with epoxy resin emulsion. The cooperation between the two can effectively improve the strength and crack resistance of gypsum mortar.
[0027] The present scheme also utilizes allyl glycidyl ether, 1,1,3,3-tetramethyldisiloxane, diethylenetriamine and other components to prepare an amino-terminated curing agent, which is then compounded with diethylenetriamine as a curing agent, and mixed with epoxy resin to prepare an epoxy resin emulsion. By adding the epoxy resin emulsion to the system, the mechanical properties of the gypsum mortar are enhanced and the water resistance is also improved. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In this embodiment, the desulfurized gypsum semi-aqueous phase is 80-85%; the particle size of the low-density polyethylene particles is 2.5-3 mm, and the density is 50-60 kg / m 3 ; The particle size of the fumed silica particles is 1.8-2.5 mm, and the density is 40-50 kg / m 3 The sepiolite fiber has a length of 6 to 8 mm, a width of 0.8 to 1 mm, and a density of 250 to 300 kg / m 3 The length of cork fiber is 2-3 mm, the width is 0.5-0.8 mm, and the density is 160-180 kg / m 3 .
[0030] The retarder is a protein-based gypsum retarder, model SG-12X, from Xingbang; the cellulose ether is hydroxypropyl methylcellulose ether, model H100, from Shandong Yiteng Cellulose Ether Co., Ltd.; the rubber powder is VAE rubber powder from Wacker Chemical (China) Co., Ltd., model 5044, and the thixotropic enzyme is magnesium aluminum silicate. The epoxy resin model is WSR-615.
[0031] The preparation steps of polyvinyl alcohol fiber are as follows: using PVA1799 as raw material, melt spinning, the temperature is 160°C, the temperature of the heating sleeve at the spinneret is 130°C, stretching and pulling, the stretching multiple is 4, and circular polyvinyl alcohol fiber or trilobal polyvinyl alcohol fiber or quadrilobal polyvinyl alcohol fiber is formed according to the difference in the shape of the holes of the spinneret; wherein the equivalent diameter of the spinneret hole is 0.3 mm, and the number of holes is 24.
[0032] Embodiment 1: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0033] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 minute, and then adding the premix additive and stirring for 3 minutes to obtain a mixture;
[0034] Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
[0035] The components of the sound insulation mortar include, by mass, 80 parts of desulfurized gypsum, 6 parts of polyethylene particles, 5.2 parts of fumed silica particles, 4.1 parts of sepiolite fiber, 4 parts of cork fiber, 0.24 parts of retarder, 0.22 parts of cellulose ether, 1.5 parts of rubber powder, 0.28 parts of thixotropic enzyme, and 44.2 parts of deionized water.
[0036] Embodiment 2: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0037] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 minute, and then adding the premix additive and stirring for 3 minutes to obtain a mixture;
[0038] Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
[0039] The components of the sound insulation mortar include, by mass, 74 parts of desulfurized gypsum, 8 parts of polyethylene particles, 7 parts of fumed silica particles, 5.8 parts of sepiolite fiber, 6.5 parts of cork fiber, 0.26 parts of retarder, 0.26 parts of cellulose ether, 1.8 parts of rubber powder, 0.32 parts of thixotropic enzyme, and 43.5 parts of deionized water.
[0040] Embodiment 3: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0041] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 minute, and then adding the premix additive and stirring for 3 minutes to obtain a mixture;
[0042] Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
[0043] The components of the sound insulation mortar include, by mass, 68 parts of desulfurized gypsum, 10 parts of polyethylene particles, 8.2 parts of fumed silica particles, 7 parts of sepiolite fiber, 7.6 parts of cork fiber, 0.3 parts of retarder, 0.3 parts of cellulose ether, 2.3 parts of rubber powder, 0.4 parts of thixotropic enzyme, and 42.5 parts of deionized water.
[0044] Embodiment 4: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0045] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 to 2 minutes, and then adding the premix additive, stirring for 3 to 5 minutes to obtain a mixture;
[0046] Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
[0047] The components of the sound insulation mortar include, by mass, 60 parts of desulfurized gypsum, 12 parts of polyethylene particles, 10 parts of fumed silica particles, 8 parts of sepiolite fiber, 10 parts of cork fiber, 0.38 parts of retarder, 0.35 parts of cellulose ether, 2.8 parts of rubber powder, 0.52 parts of thixotropic enzyme, and 40 parts of deionized water.
[0048] Embodiment 5: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0049] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 to 2 minutes, and then adding the premix additive, stirring for 3 to 5 minutes to obtain a mixture;
[0050] Step (2): Mix the epoxy resin emulsion and the pretreated polyvinyl alcohol fiber, stir evenly to obtain a polymer solution; mix the mixture, the polymer solution and deionized water, stir evenly to obtain a sound insulation mortar.
[0051] The components of the sound insulation mortar include: by weight, 68 parts of desulfurized gypsum, 10 parts of polyethylene particles, 8.2 parts of fumed silica particles, 7 parts of sepiolite fiber, 7.6 parts of cork fiber, 0.3 parts of retarder, 0.3 parts of cellulose ether, 2.3 parts of rubber powder, 0.4 parts of thixotropic enzyme, and 42.5 parts of deionized water. The amount of the epoxy resin emulsion accounts for 4wt% of the total mass of the desulfurized gypsum; the pretreated polyvinyl alcohol fiber accounts for 1wt% of the total mass of the desulfurized gypsum.
[0052] The preparation steps of the pretreated polyvinyl alcohol fiber are as follows: 2.5 mL of concentrated nitric acid and 37.5 mL of deionized water are mixed, 1.5 g of ammonium cerium nitrate is added, and the mixture is stirred evenly to obtain an ammonium cerium nitrate solution; 400 mL of deionized water, 10 g of polyvinyl alcohol fiber and 20.5 g of glycidyl methacrylate are mixed, and ultrasonic dispersion is performed for 25 minutes to obtain a dispersion; 40 mL of ammonium cerium nitrate solution is added to the dispersion, and the mixture is reacted at 45° C. for 6 hours, and the product is collected by filtration, washed and dried to obtain the pretreated polyvinyl alcohol fiber; the polyvinyl alcohol fiber is a compound of trilobal polyvinyl alcohol fiber and quadrilobal polyvinyl alcohol fiber, and the mass ratio is 2:3. The concentration of the concentrated nitric acid is 16 mol / L.
[0053] The preparation steps of epoxy resin emulsion are:
[0054] S1: Heat allyl glycidyl ether to 65°C, add chloroplatinic acid-isopropanol mixture, stir for 10 minutes, slowly drop 1,1,3,3-tetramethyldisiloxane, keep warm for 2.5 hours, collect the product after cooling, and obtain epoxy silane; the molar ratio of allyl glycidyl ether to 1,1,3,3-tetramethyldisiloxane is 2.4:1.
[0055] Epoxysilane and diethylenetriamine were mixed, heated to 75° C., and kept warm for 6 hours to obtain an amino-terminated curing agent; the molar ratio of the epoxysilane to diethylenetriamine was 1:1.8.
[0056] S2: Mix the amino-terminated curing agent and diethylenetriamine, stir evenly to obtain a compound curing agent; mix the epoxy resin and the compound curing agent, stir for 30 minutes, and obtain an epoxy resin emulsion. The mass ratio of the amino-terminated curing agent and diethylenetriamine is 4:1; the mass ratio of the epoxy resin and the compound curing agent is 4:1.
[0057] Embodiment 6: A preparation process of gypsum floor sound insulation mortar, the specific steps are:
[0058] Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 to 2 minutes, and then adding the premix additive, stirring for 3 to 5 minutes to obtain a mixture;
[0059] Step (2): Mix the epoxy resin emulsion and the pretreated polyvinyl alcohol fiber, stir evenly to obtain a polymer solution; mix the mixture, the polymer solution and deionized water, stir evenly to obtain a sound insulation mortar.
[0060] The components of the sound insulation mortar include: by weight, 60 parts of desulfurized gypsum, 12 parts of polyethylene particles, 10 parts of fumed silica particles, 8 parts of sepiolite fiber, 10 parts of cork fiber, 0.38 parts of retarder, 0.35 parts of cellulose ether, 2.8 parts of rubber powder, 0.52 parts of thixotropic enzyme, and 40 parts of deionized water. The amount of the epoxy resin emulsion accounts for 5wt% of the total mass of the desulfurized gypsum; the pretreated polyvinyl alcohol fiber accounts for 1.5wt% of the total mass of the desulfurized gypsum.
[0061] The preparation steps of the pretreated polyvinyl alcohol fiber are as follows: 2.5 mL of concentrated nitric acid and 37.5 mL of deionized water are mixed, 1.5 g of ammonium cerium nitrate is added, and the mixture is stirred evenly to obtain an ammonium cerium nitrate solution; 400 mL of deionized water, 10 g of polyvinyl alcohol fiber and 20.5 g of glycidyl methacrylate are mixed, and ultrasonic dispersion is performed for 25 minutes to obtain a dispersion; 40 mL of ammonium cerium nitrate solution is added to the dispersion, and the mixture is reacted at 45° C. for 6 hours, and the product is collected by filtration, washed and dried to obtain the pretreated polyvinyl alcohol fiber; the polyvinyl alcohol fiber is a compound of trilobal polyvinyl alcohol fiber and quadrilobal polyvinyl alcohol fiber, and the mass ratio is 2:3. The concentration of the concentrated nitric acid is 16 mol / L.
[0062] The preparation steps of epoxy resin emulsion are:
[0063] S1: Heat allyl glycidyl ether to 65°C, add chloroplatinic acid-isopropanol mixture, stir for 10 minutes, slowly drop 1,1,3,3-tetramethyldisiloxane, keep warm for 2.5 hours, collect the product after cooling, and obtain epoxy silane; the molar ratio of allyl glycidyl ether to 1,1,3,3-tetramethyldisiloxane is 2.4:1.
[0064] Epoxysilane and diethylenetriamine were mixed, heated to 75° C., and kept warm for 6 hours to obtain an amino-terminated curing agent; the molar ratio of the epoxysilane to diethylenetriamine was 1:1.8.
[0065] S2: Mix the amino-terminated curing agent and diethylenetriamine, stir evenly to obtain a compound curing agent; mix the epoxy resin and the compound curing agent, stir for 30 minutes, and obtain an epoxy resin emulsion. The mass ratio of the amino-terminated curing agent and diethylenetriamine is 4:1; the mass ratio of the epoxy resin and the compound curing agent is 4:1.
[0066] Comparative Example 1: An ordinary sound insulation mortar, the specific preparation steps are: according to 25 parts of cement, 15 parts of fly ash, 10 parts of perlite, 50 parts of sand, 0.2 parts of cellulose ether, 1.2 parts of glue powder, add 35 parts of deionized water, mix well to obtain ordinary sound insulation mortar.
[0067] Comparative Example 2: Taking Example 6 as the control group, the polyvinyl alcohol fibers used in the pretreatment were round polyvinyl alcohol fibers, and the other steps remained unchanged.
[0068] The dosage of each component in Examples 1 to 4 and Comparative Example 1 is shown in Table 1 below:
[0069] Table 1
[0070] Components / mass Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Desulfurization gypsum 80 74 68 60 68 60 Polyethylene granules 6 8 10 12 10 12 Fumed silica particles 5.2 7 8.2 10 8.2 10 Sepiolite Fiber 4.1 5.8 7 8 7 8 Cork fiber 4 6.5 7.6 10 7.6 10 Retarder 0.24 0.26 0.3 0.38 0.3 0.38 Cellulose ether 0.22 0.26 0.3 0.35 0.3 0.35 Rubber powder 1.5 1.8 2.3 2.8 2.3 2.8 Thixotropic enzyme 0.28 0.32 0.4 0.52 0.4 0.52 Deionized water 44.2 43.5 42.5 40 42.5 40 Epoxy resin emulsion / / / / 4wt% 5wt% Polyvinyl alcohol fiber / / / / 1wt% 1.5wt%
[0071] In the two rows of epoxy resin emulsion and polyvinyl alcohol fiber, wt% refers to the mass percentage of the component in the total mass of desulfurized gypsum.
[0072] Detection experiment:
[0073] The sound insulation mortars prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested for tensile bonding strength and density according to the method disclosed in JGJ70-2009; the impact improvement volume was tested according to GB / T50121-2005 "Building Sound Insulation Evaluation Standard"; the water absorption was tested according to the method disclosed in JG / T698-2010, and the mortars were soaked in 23°C water for 24 hours, and the surface was wiped dry after being taken out, and the mortars were weighed and the water absorption was calculated; the specific test data are shown in Table 2 below:
[0074] Table 2
[0075]
[0076] Conclusion: From the comparison of Examples 1 to 4 above, it can be seen that with the increase of sound insulation materials such as polyethylene particles, fumed silica particles, sepiolite fibers, and cork fibers, the density of the sound insulation mortar gradually decreases, the sound insulation improvement gradually increases, and the sound insulation effect is better; from the comparison of Examples 5 to 6 and Comparative Examples 1 to 2, it can be seen that after the addition of polyvinyl alcohol fibers and epoxy resin emulsion, the mechanical properties, water absorption rate and sound insulation performance of the mortar are improved.
[0077] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A gypsum floor sound insulation mortar, characterized in that: The components of the sound insulation mortar include, by mass, 60-80 parts of desulfurized gypsum, 6-12 parts of polyethylene particles, 5-10 parts of fumed silica particles, 4-8 parts of sepiolite fibers, 4-10 parts of cork fibers, 0.2-0.45 parts of retarder, 0.2-0.5 parts of cellulose ether, 1.5-3 parts of rubber powder, 0.2-0.6 parts of thixotropic enzyme, and 40-45 parts of deionized water.
2. The gypsum floor sound insulation mortar according to claim 1, characterized in that: The desulfurized gypsum semi-aqueous phase is 80-85%; the particle size of the polyethylene particles is 2.5-3mm; the particle size of the fumed silica particles is 1.8-2.5mm; the length of the sepiolite fiber is 6-8mm, and the width is 0.8-1mm; the length of the cork fiber is 2-3mm, and the width is 0.5-0.8mm.
3. The gypsum floor sound insulation mortar according to claim 1, characterized in that: The retarder is a protein-based gypsum retarder; the cellulose ether is hydroxypropyl methylcellulose ether; the rubber powder is VAE rubber powder, and the thixotropic enzyme is a magnesium aluminum silicate lubricant.
4. The gypsum floor sound insulation mortar according to claim 1, characterized in that: The sound insulation mortar also includes epoxy resin emulsion and pretreated polyvinyl alcohol fiber. The epoxy resin emulsion accounts for 4-6wt% of the total mass of the desulfurized gypsum; the pretreated polyvinyl alcohol fiber accounts for 0.5-2.5wt% of the total mass of the desulfurized gypsum.
5. The gypsum floor sound insulation mortar according to claim 4, characterized in that: The preparation steps of the pretreated polyvinyl alcohol fiber are as follows: mixing concentrated nitric acid and deionized water, adding ammonium cerium nitrate, stirring evenly to obtain an ammonium cerium nitrate solution; mixing deionized water, polyvinyl alcohol fiber and glycidyl methacrylate, and ultrasonically dispersing for 20 to 30 minutes to obtain a dispersion; adding 40 mL of the ammonium cerium nitrate solution to the dispersion, reacting at 40 to 45° C. for 5 to 6 hours, filtering and collecting the product, washing and drying to obtain the pretreated polyvinyl alcohol fiber; The polyvinyl alcohol fiber is any one or more of trilobal polyvinyl alcohol fiber, quadrilobal polyvinyl alcohol fiber, triangular polyvinyl alcohol fiber and circular polyvinyl alcohol fiber.
6. The gypsum floor sound insulation mortar according to claim 5, characterized in that: The polyvinyl alcohol fiber is a compound of trilobal polyvinyl alcohol fiber and quadrilobal polyvinyl alcohol fiber, with a mass ratio of 2:
3.
7. The gypsum floor sound insulation mortar according to claim 4, characterized in that: The preparation steps of the epoxy resin emulsion are: S1: Heat allyl glycidyl ether to 60-65°C, add chloroplatinic acid-isopropanol mixture, stir for 10-20 minutes, slowly drop 1,1,3,3-tetramethyldisiloxane, keep warm for 2-2.5 hours, cool and collect the product to obtain epoxysilane; Mix epoxy silane and diethylenetriamine, raise the temperature to 70-75°C, and keep the temperature to react for 5-6 hours to obtain an amino-terminated curing agent; S2: Mix the amino-terminated curing agent and diethylenetriamine, stir evenly to obtain a compound curing agent; mix the epoxy resin and the compound curing agent, stir for 20 to 30 minutes, and obtain an epoxy resin emulsion.
8. The gypsum floor sound insulation mortar according to claim 7, characterized in that: In S1, the molar ratio of allyl glycidyl ether to 1,1,3,3-tetramethyldisiloxane is (2.1-2.4):1; the molar ratio of epoxysilane to diethylenetriamine is 1:(1.5-2); In S2, the mass ratio of the amino-terminated curing agent to diethylenetriamine is (4-5):1; the mass ratio of the epoxy resin to the compound curing agent is (3-4):
1.
9. A preparation process for gypsum floor sound insulation mortar, characterized in that: The specific steps are: Step (1): mixing a retarder, cellulose ether, rubber powder and thixotropic enzyme, stirring evenly to obtain a premix additive; mixing desulfurized gypsum, polyethylene particles, fumed silica particles, sepiolite fibers and cork fibers, stirring for 1 to 2 minutes, and then adding the premix additive, stirring for 3 to 5 minutes to obtain a mixture; Step (2): Mix the mixture and deionized water, mix evenly, and obtain sound insulation mortar.
10. The preparation process of the gypsum floor sound insulation mortar according to claim 9, characterized in that: Step (2) specifically comprises: mixing the epoxy resin emulsion and the pretreated polyvinyl alcohol fiber, stirring evenly to obtain a polymer solution; mixing the admixture, the polymer solution and deionized water, stirring evenly to obtain a sound insulation mortar.