Preparation method of MEMS pressure chip

Through the combination of SOI wafer and silicon oxide pattern layer, wet corrosion and photolithography technology are used to form the island-shaped structure of the MEMS pressure chip, which solves the problem of large island structure and limited design freedom in the existing technology, and realizes the chip Size reduction and shape diversified design.

CN118954425APending Publication Date: 2024-11-15NORTH ELECTRON RES INST ANHUI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318882.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The island structure in the existing MEMS pressure chip process is large, which leads to a larger chip size, making it difficult to form beam and island structures of various shapes, and the degree of freedom of the structure size and thickness design is limited.

Method used

The combination of SOI wafer and silicon oxide pattern layer is used to form a groove body, cavity and island structure through wet corrosion and lithography processes to realize the preparation of MEMS pressure chips, allowing chip size reduction and structural shape diversified design.

Benefits of technology

The size reduction of the MEMS pressure chip island structure is achieved, allowing the formation of shapes that are difficult to achieve in conventional processes, and maximizing the freedom of structural design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954425A_ABST
    Figure CN118954425A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an MEMS pressure chip. The preparation method is characterized by comprising the steps that a silicon oxide pattern layer is prepared on a first SOI wafer, the first SOI wafer and the second SOI wafer are bonded together, an upper oxide layer, a piezoresistor, a lead and a second cavity are arranged on the first SOI wafer, and a lower oxide layer, a groove body and a cavity are arranged on the second SOI wafer. According to the preparation scheme provided by the invention, the size of the back island structure of the MEMS pressure chip can be reduced by many times compared with a conventional process, the size of the chip can be greatly reduced, meanwhile, beam and island structures in various shapes which are difficult to form by the conventional process can be formed by the preparation process, the size and thickness of the structure can be freely designed, and the production cost is reduced. And the degree of freedom of design is maximized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field: The invention relates to the field of MEMS process manufacturing, and in particular to a method for preparing a MEMS pressure chip. Background technology: The pressure sensitive element of the MEMS pressure sensor is the MEMS pressure chip. The MEMS pressure chip is generally formed into a flat film, an island film or a beam film structure on a silicon substrate through processes such as film formation, photolithography and etching. The flat film and island film structures are formed by using a surface patterned dielectric layer behind the wafer as an etching mask and then etching the silicon substrate with KOH or TMAH solution. The problem is that the island structure made by conventional processes is large, resulting in a larger chip size, making it difficult to form beams and island structures of various shapes by etching, and the size and thickness of the structure cannot be freely designed. Summary of the invention: The present invention is to overcome the deficiencies in the prior art and provide a method for preparing a MEMS pressure chip, thereby overcoming the problems in the prior art of large island structure and chip size, and limited design freedom of structure shape, size and thickness.

[0004] This application provides the following technical solutions: A method for preparing a MEMS pressure chip, characterized in that it comprises the following steps: S1, preparing a first SOI wafer and a second SOI wafer; S2, preparing a patterned silicon oxide layer on the upper surface of the first SOI wafer by oxidation; S3, secondly, forming a groove on the upper surface of the SOI wafer by wet etching; S4, bonding the silicon oxide pattern layer to the upper surface of the second SOI wafer; S5, removing the substrate silicon and buried oxide layer of the first SOI wafer and the second SOI wafer; S6, forming an upper and a lower oxide layer on the top silicon upper surface of the first SOI wafer and the second SOI wafer, preparing a group of varistors on the top silicon by photolithography and implantation processes on the upper oxide layer, and providing a lead electrically connected to each varistor on the upper oxide layer; S7, forming a cavity connected to the groove body upward on the lower oxide layer of the top silicon of the second SOI wafer by wet etching; S8, then continue to wet-etch upward through the gaps between the silicon oxide pattern layers to form a second cavity on the top silicon layer of the first SOI wafer for a distance, so that the top silicon layer of the first SOI wafer between two adjacent second cavities forms an island structure, thereby manufacturing a MEMS pressure chip.

[0005] On the basis of the above technical solutions, there are also the following further technical solutions: When the first SOI wafer 1 is oxidized in S2, the thickness of the oxide layer is calculated based on the corrosion depth of silicon in the "silicon-silicon oxide" wet etching of KOH solution or TMAH solution, wherein the corrosion rate ratio is 98:1 to 102:1 when using KOH solution, and the corrosion rate ratio is 8000:1 to 8500:1 when using TMAH solution.

[0006] In the step S1, the sum of the thickness of the top silicon layers of the first SOI wafer and the second SOI wafer is not less than 350 μm.

[0007] In step S5, mechanical thinning and etching are used in sequence to thin the SOI wafer and the substrate silicon of the SOI wafer, and then the buried oxide layers of the two are removed through the BOE process.

[0008] In step S6, the thickness of the upper and lower oxide layers is 0.05 μm-0.1 μm, and the aluminum lead is manufactured by sequentially performing sputtering, photolithography and etching processes.

[0009] In steps S3, S7 and S8, the wet etching is carried out by using KOH or TMAH solution.

[0010] Advantages of the invention: The preparation scheme provided by the present invention enables the size of the island structure on the back side of the MEMS pressure chip to be reduced many times compared with conventional processes, and the chip size can also be greatly reduced. At the same time, the preparation process can also form beams and island structures of various shapes that are difficult to form with conventional processes. The size and thickness of the structure can be freely designed, thereby maximizing the design freedom. Description of the drawings: Figure 1 This is a schematic diagram of the structure after step S2 of the present invention is completed; Figure 2 This is a schematic diagram after S3 is completed; Figure 3 This is the schematic diagram after S4 is completed; Figure 4 This is the schematic diagram after S5 is completed; Figure 5 This is the schematic diagram of S6 after completion; Figure 6 This is the schematic diagram of S7 after completion; Figure 7 This is a schematic diagram of the structure of the MEMS pressure chip produced after S7 is completed. Specific implementation method: like Figure 1-7 As shown, a method for preparing a MEMS pressure chip comprises the following steps: S1. Prepare a first SOI wafer 1 and a second SOI wafer 2. Both SOI wafers include a top silicon a, a buried oxide layer b and a substrate silicon c which are sequentially distributed from top to bottom.

[0013] S2. A patterned silicon oxide pattern layer 111 is prepared on the upper surface of the top silicon layer of the SOI wafer 1 by thermal oxidation. During the oxidation, a KOH solution is used for wet etching, and the etching rate ratio is 100:1.

[0014] S3 , forming a groove 211 on the top silicon surface of the second SOI wafer 2 by wet etching.

[0015] S4 , turning over the first SOI wafer 1 , and then bonding the silicon oxide pattern layer 111 to the top silicon upper surface of the second SOI wafer 2 .

[0016] S5, removing the substrate silicon and buried oxide layer of the first SOI wafer 1 and the second SOI wafer 2; S6, an upper oxide layer 114 and a lower oxide layer 115 are formed on the upper surfaces of the top silicon layers a of the first SOI wafer 1 and the second SOI wafer 2. The thickness of the upper oxide layer 114 and the lower oxide layer 115 is 0.07 μm.

[0017] A group of varistors 112 are fabricated on the top silicon layer through photolithography and implantation processes on the upper oxide layer 114. The varistors 112 include a P+ region 112a and a P- region 112b heavily doped with boron.

[0018] A contact hole 1114 is formed on the upper oxide layer 114 by etching, and then an aluminum lead 113 is prepared on the upper oxide layer 114 by sputtering, photolithography and etching processes in sequence, and a part of the lead 113 fills the contact hole 1114 and forms an electrical connection with the P+ region 112a, thereby achieving electrical connection with the varistor 112. The P+ region 112a is easy to form an ohmic contact with the metal lead, and plays a good electrical connection role.

[0019] S7. On the lower oxide layer 115 of the top silicon of the second SOI wafer 2, a KOH solution is used to form a cavity 22 connected to the groove body 211 upward by wet etching, and an opening is provided below the cavity 22, so that a through hole penetrating the top silicon of the second SOI wafer 2 is formed through the groove body 211 and the cavity 22.

[0020] S8. After the cavity 22 is formed, the top silicon a of the first SOI wafer 1 is continuously wet-etched upward for a distance through the gap between the silicon oxide pattern layers 111, and then a second cavity 117 connected to the cavity 22 is formed, so that the top silicon of the first SOI wafer 1 between two adjacent second cavities 117 forms an island structure 116, and the remaining top silicon a of the first SOI wafer 1 above the second cavity 117 forms a beam structure, thereby manufacturing a MEMS pressure chip.

[0021] A MEMS pressure chip prepared by the above preparation method includes a top silicon layer of an SOI wafer 1, on the top layer of the SOI wafer 1, a patterned silicon oxide pattern layer 111 and a second cavity 117 are provided, and an upper oxide layer 114 is provided on the other side.

[0022] A group of varistors 112 is disposed on the top silicon layer of the SOI wafer 1 below the upper oxide layer 114 , and metal leads 113 correspondingly connected to the varistors 112 are disposed above the upper oxide layer 114 .

[0023] The top silicon layer of the second SOI wafer 2 is connected to the silicon oxide graphic layer 111, a groove body 211 is provided on the top silicon layer of the second SOI wafer 2, a lower oxide layer 115 is provided on the lower surface of the top silicon layer of the second SOI wafer 2, an upward cavity 22 is provided on the lower oxide layer 115, and the cavity 22, the groove body 211 and the second cavity 117 are connected.

Claims

1. A method for preparing a MEMS pressure chip, characterized in that: It includes the following steps: S1, preparing a first SOI wafer (1) and a second SOI wafer (2); S2, preparing a patterned silicon oxide pattern layer (111) on the upper surface of the first SOI wafer (1) by oxidation; S3, forming a groove body (211) on the upper surface of the second SOI wafer (2) by wet etching; S4, bonding the silicon oxide pattern layer (111) to the upper surface of the second SOI wafer (2); S5, removing the substrate silicon and buried oxide layer of the SOI wafer (1) and the second SOI wafer (2); S6. Upper and lower oxide layers (114, 115) are formed on the top silicon surfaces of the first SOI wafer (1) and the second SOI wafer (2), a group of varistors (112) are prepared on the top silicon of the upper oxide layer (114) by sequentially performing photolithography and implantation processes, and leads (113) are provided on the upper oxide layer (114) to form an electrical connection with each varistor (112); S7, forming a cavity (22) communicating with the groove body (211) upwardly on the lower oxide layer (115) of the top silicon of the second SOI wafer 2 by wet etching; S8, then continuing to wet-etch upwards through the gaps between the silicon oxide pattern layers (111) to form a second cavity (117) at one end of the top silicon layer of the first SOI wafer (1), so that the top silicon layer of the first SOI wafer (1) between two adjacent second cavities (117) forms an island structure (116), thereby manufacturing a MEMS pressure chip.

2. The method for preparing a MEMS pressure chip according to claim 1, characterized in that: When the SOI wafer 1 is oxidized in S2, the thickness of the oxide layer is calculated based on the corrosion depth of silicon in the "silicon-silicon oxide" wet etching of KOH solution or TMAH solution, wherein the corrosion rate ratio is 98:1 to 102:1 when using KOH solution, and the corrosion rate ratio is 8000:1 to 8500:1 when using TMAH solution.

3. The method for preparing a MEMS pressure chip according to claim 1, characterized in that: In the step S1, the sum of the thickness of the top silicon layers of the first SOI wafer (1) and the second SOI wafer (2) is not less than 350 μm.

4. The method for preparing a MEMS pressure chip according to claim 1, characterized in that: In step S5, the substrate silicon of the first SOI wafer (1) and the SOI wafer (2) are thinned by mechanical thinning and etching in sequence, and then the buried oxide layers of the two are removed by BOE process.

5. The method for preparing a MEMS pressure chip according to claim 1, characterized in that: In step S6, the thickness of the upper and lower oxide layers (114, 115) is 0.05 μm-0.1 μm, and the aluminum lead (113) is manufactured by sequentially performing sputtering, photolithography and etching processes.

6. The method for preparing a MEMS pressure chip according to claim 1, characterized in that: In steps S3, S7 and S8, the wet etching is carried out by using KOH or TMAH solution.