Hard carbon negative electrode material and preparation method and application thereof
By pickling, oxidation and solidification of the carbon source precursor of the hard carbon anode material of sodium ion battery, combined with pyrolysis and high-temperature carbonization, the problems of uneven oxidation and slow melt mass transfer are solved, and sodium storage and magnification are improved Performance, achieving easy operation and low cost hard carbon material preparation.
Patent Information
- Application Number
- CN202411047788.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-01
AI Technical Summary
In the prior art, when preparing sodium ion battery hard carbon anode materials, the problems of uneven oxidation and slow melt mass transfer rate lead to limited sodium storage capacity and rate performance.
By acid-eluting ash, oxidation curing and deep oxidation on the carbon source precursor, the degree of oxidation and crosslinking are improved, combined with pyrolysis and high-temperature carbonization, a disorderly distributed amorphous hard carbon material is formed, and the crystal plane spacing is increased to increase the distance between the crystals to improve the The intercalation capacity of sodium ions.
It improves the sodium storage performance and rate performance of the negative electrode material, is easy to operate, has low raw material and process costs, and has a wide range of applications.
Smart Images

Figure CN118954478A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery electrode materials and relates to a hard carbon negative electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are currently widely used in mobile electronic devices, new energy vehicles, power tools, and other fields due to their high energy density and excellent safety performance. However, the limited and expensive lithium resources have limited the application of lithium-ion batteries in large-scale energy storage systems. Compared to lithium, sodium resources are abundant in the Earth's crust and are relatively cheap. Therefore, sodium-ion batteries have broad application prospects in large-scale energy storage systems and are expected to be used in the next generation of large-scale energy storage devices.
[0003] Because sodium ions have a larger radius than lithium ions, they are difficult to fit into the interlayer spacing of graphite anodes, making graphite unsuitable as anode materials for sodium-ion batteries. This makes anode materials one of the main issues hindering the development of lithium-ion batteries. Amorphous carbon materials, due to their low degree of graphitization, high degree of disorder, and large interlayer spacing, have high sodium storage capacity and hold great promise as anode materials for sodium-ion batteries.
[0004] Hard carbon, as a type of amorphous carbon material, has a disordered and curved carbon layer. It can store sodium in a variety of ways such as intercalation, adsorption and pore filling, and has a high capacity. Its raw materials mainly come from various carbon sources, including polymer compounds, biomass, organic matter, etc., among which commonly used organic matter includes asphalt, coal, etc. However, direct carbonization of raw materials such as asphalt usually forms soft carbon materials with high order, small interplanar spacing, and low sodium storage capacity. Therefore, the organic carbon source needs to be modified to form a cross-linked structure to increase the disorder and interplanar spacing of the carbon layer. However, due to the different types of carbon source precursors, conventional modification methods are difficult to apply universally.
[0005] CN 115991467A discloses an oxidized asphalt-based hard carbon negative electrode material for sodium ion batteries and its preparation method. The method comprises: crushing asphalt, adjusting the temperature using a fluidized bed, oxidizing the crushed asphalt to obtain an oxidized precursor, and then sieving and carbonizing the oxidized asphalt to obtain an oxidized asphalt-based hard carbon negative electrode material. CN 109148883A discloses an asphalt-based sodium ion battery negative electrode material and its preparation method and application. The method comprises: pre-oxidizing the asphalt precursor at 200-350°C for 2-6 hours, then placing it in a high-temperature carbonization furnace, heating it to 1300-1600°C at a heating rate of 0.5-5°C / min, and heat-treating it in an inert atmosphere for 1-10 hours to carbonize and crack the pre-oxidized asphalt, and then cooling it to room temperature to obtain an irregular, amorphous carbon material. The above patents all involve oxidative modification of asphalt, which deepens the degree of oxidation of the asphalt, breaks the ordered structure of the asphalt, and increases the degree of cross-linking. However, there are still problems of slow mass transfer rate after melting and uneven oxidation. The amorphous carbon formed still contains a large amount of long-range, ordered carbon layer structure and a low interlayer spacing, resulting in limited capacity after carbonization.
[0006] CN 116553512A discloses a method for preparing a hard carbon material for sodium ion batteries. The method comprises: uniformly mixing an asphalt-based material with a sulfur-containing compound to obtain a first mixed precursor; pressing the mixture into sheets; heat-treating the mixture in an oxidizing atmosphere; cooling the mixture to obtain a cross-linked modified asphalt; and uniformly mixing the mixture with a pore-forming agent and a pore modifier to obtain a second mixed precursor. The mixture is then calcined in an inert atmosphere or a hydrocarbon atmosphere; cooled; ground; acid-washed; washed; and dried to obtain an amorphous sodium ion battery negative electrode material. Although this method also uses an asphalt-based material as a raw material and similarly involves oxidation and calcination and carbonization of the asphalt, it still suffers from uneven oxidation and slow mass transfer after melting. Furthermore, the method utilizes multiple components, complicating the process and increasing costs.
[0007] In summary, for the preparation process of hard carbon negative electrode materials, it is necessary to adopt a suitable pre-oxidation process according to the selection of raw material precursors to improve the uniformity of oxidation, obtain an ideal cross-linked structure, and improve the sodium storage capacity and rate performance of the negative electrode material. Summary of the Invention
[0008] In response to the problems existing in the prior art, the purpose of the present invention is to provide a hard carbon negative electrode material, a preparation method and use thereof. The method performs oxidative curing and deep oxidation on the carbon source precursor to increase the oxidation degree and cross-linking degree of the precursor, and then combines pyrolysis and high-temperature carbonization to increase the disorder and interplanar spacing of the carbon layer, thereby obtaining a hard carbon negative electrode material, effectively improving the sodium storage capacity and improving the rate performance.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a method for preparing a hard carbon negative electrode material, the preparation method comprising the following steps:
[0011] (1) acid-washing and deashing the carbon source precursor, and then sequentially performing oxidative curing and deep oxidation in an oxygen-containing atmosphere, wherein the oxidative curing temperature is lower than the deep oxidation temperature, to obtain an oxidized precursor;
[0012] (2) The oxidized precursor obtained in step (1) is subjected to pyrolysis and high-temperature carbonization in an inert atmosphere to obtain a hard carbon negative electrode material.
[0013] In the present invention, for the preparation of sodium ion battery negative electrode materials, it is necessary to increase the disorder of the carbon layer as much as possible to facilitate the embedding of sodium ions. Therefore, in the present invention, the carbon source precursor is first pickled to remove inorganic impurity components, and then pre-oxidized in an oxygen-containing atmosphere. The oxidation process is specifically divided into two stages: oxidation curing and deep oxidation. The temperature of the former is lower than that of the latter. Before the precursor melts, oxidation is performed once to increase the molecular weight of the raw material and increase its softening temperature, avoiding the problems of slow mass transfer rate and uneven oxidation caused by melting when directly oxidizing at a higher temperature. Then, deep oxidation cross-linking is performed at a higher temperature to obtain an oxidized precursor with a high degree of oxidation and a complex cross-linked structure. After thermal decomposition to remove volatiles and high-temperature carbonization treatment, a disordered amorphous hard carbon material can be formed, and the interplanar spacing is increased, which is conducive to the embedding of sodium ions, thereby improving the sodium storage performance of the negative electrode material, and excellent capacity and rate performance. The method is simple to operate, has low raw material and process costs, and has a wide range of applications.
[0014] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0015] As a preferred technical solution of the present invention, the carbon source precursor in step (1) includes any one of coal tar pitch, petroleum pitch, coal or heavy carbon, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of coal tar pitch and coal, a combination of coal and heavy carbon, a combination of coal tar pitch, petroleum pitch and coal, etc.
[0016] In the present invention, in the selection of the carbon source precursor, in addition to the above two types of asphalt, coal can be selected from bituminous coal, lignite, sub-bituminous coal, coking coal or anthracite, etc., and heavy carbon can be selected from liquefied residue, oil shale, heavy petroleum, oil sands, biomass or petroleum coke, etc. The above carbon source precursors can be used alone or in combination of two or more.
[0017] Preferably, the carbon source precursor in step (1) is first crushed and sieved to obtain raw material particles.
[0018] Preferably, the comminution includes crushing and grinding in sequence, and the crushing is followed by drying and then grinding.
[0019] Preferably, the particle size of the raw material particles selected by the screening is 3 to 20 μm, for example, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable. The above-mentioned point values of particle size generally represent the particle size of a single particle or the average value of the particle size of the raw material particles. For a certain amount of raw material particles, the particle size usually has a certain range of values, for example, 3 to 5 μm, 4 to 8 μm, 5 to 10 μm, 3 to 15 μm, 3 to 10 μm or 8 to 20 μm, etc.
[0020] Preferably, the sieved raw material particles are dried and then acid washed and deashed.
[0021] In the present invention, the carbon source precursor is first crushed and screened to reduce the particle size, increase the specific surface area, and facilitate the subsequent oxidant carbonization process; the crushing is performed using a crusher, such as a jaw crusher, and dried in a blast drying oven, the drying temperature of which can be selected at 100-120°C, and then ground by a crusher, screened by a standard vibrating screen, and the screened raw material with a particle size of 3-20 μm is selected, and then dried at 100-120°C for 3-5 hours.
[0022] As a preferred technical solution of the present invention, the acid solution used for pickling and deashing in step (1) includes hydrochloric acid and / or hydrofluoric acid, and preferably, hydrochloric acid is used for washing first, and then hydrofluoric acid is used for washing.
[0023] In the present invention, the role of the acid washing is mainly to remove inorganic components in the carbon source precursor, wherein the role of hydrochloric acid is to remove metal salts, and the role of hydrofluoric acid is to remove aluminosilicates.
[0024] Preferably, the carbon source precursor is mixed with hydrochloric acid and then stirred for washing, allowed to stand, washed with water, filtered, and dried to obtain a first acid-washed raw material.
[0025] Preferably, the solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1g:(2-10)mL, for example 1g:2mL, 1g:3mL, 1g:4mL, 1g:5mL, 1g:6mL, 1g:7mL, 1g:8mL, 1g:9mL or 1g:10mL, etc., but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 1g:(2-4)mL.
[0026] Preferably, the mass fraction of the hydrochloric acid is 10-37%, for example, 10%, 15%, 20%, 25%, 30%, 35% or 37%, etc., but is not limited to the listed values. Other values not listed within this numerical range are also applicable, preferably 30-37%.
[0027] In the present invention, the carbon source precursor after crushing and screening is mixed with hydrochloric acid, stirred at a speed of 80 to 120 r / min for 10 to 15 hours, then allowed to stand for 1 to 3 hours, and repeatedly washed with distilled water until there is no Cl - After filtering, it is dried in a blast drying oven at 100-120°C for 10-15 hours to obtain the demineralized raw material.
[0028] Preferably, the first pickling raw material is mixed with hydrofluoric acid, stirred and washed, allowed to stand, washed with water, filtered, and dried to obtain the second pickling raw material.
[0029] Preferably, the solid-liquid ratio of the first pickling raw material to hydrofluoric acid is 1g:(1-10)mL, for example 1g:1mL, 1g:2mL, 1g:3mL, 1g:4mL, 1g:5mL, 1g:6mL, 1g:7mL, 1g:8mL, 1g:9mL or 1g:10mL, etc., but is not limited to the enumerated values. Other unlisted values within the numerical range are also applicable, preferably 1g:(1-3)mL.
[0030] Preferably, the mass fraction of the hydrofluoric acid is 25-40%, for example, 25%, 27%, 30%, 32%, 35%, 38% or 40%, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0031] In the present invention, the first pickling raw material is mixed with hydrofluoric acid and stirred at a speed of 80 to 120 r / min for 20 to 28 hours, then allowed to stand for 2 to 4 hours, filtered and washed with distilled water for multiple washings until there is no F - , and then dried in a blast drying oven at 100-120°C for 10-15h to obtain the acid-washed raw material.
[0032] As a preferred technical solution of the present invention, the concentration of oxygen in the oxygen-containing atmosphere in step (1) is 10% to 100%, for example, 10%, 21%, 30%, 40%, 50%, 60%, 80% or 100%, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0033] Preferably, the concentration of the oxygen-containing atmosphere in step (1) is independently selected during oxidative curing and deep oxidation, and is preferably the same concentration.
[0034] Preferably, the oxidative curing and deep oxidation in step (1) are both carried out in a tube furnace, preferably in a constant temperature zone of the tube furnace.
[0035] Preferably, the oxidative curing and deep oxidation in step (1) are carried out consecutively, and after the oxidative curing is completed, the temperature is continued to be raised for deep oxidation.
[0036] As a preferred technical solution of the present invention, the temperature of the oxidative curing in step (1) is lower than the softening point of the carbon source precursor or the temperature corresponding to the maximum weight when thermogravimetry is selected.
[0037] Preferably, the temperature of the oxidative curing in step (1) is 70-320°C, for example, 70°C, 100°C, 150°C, 200°C, 250°C, 270°C, 300°C or 320°C, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the time is 1-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the heating rate is 0.2-5°C / min, for example, 0.2°C / min, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 4°C / min or 5°C / min, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0038] In the present invention, different temperatures are selected for the oxidative curing according to the different types of carbon source precursors. When asphalt is selected as the carbon source precursor, the temperature of oxidative curing is generally selected to be about 10°C lower than the softening point. When coal or heavy carbon is selected, the temperature of oxidative curing is generally selected to be the temperature corresponding to the maximum weight value in the thermogravimetric curve. This is because the reaction activity of the precursor is the strongest at this temperature.
[0039] Preferably, the temperature of the deep oxidation in step (1) is 120-360°C, for example, 120°C, 150°C, 200°C, 250°C, 270°C, 300°C, 320°C, 350°C or 360°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the time is 1-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the heating rate is 0.2-5°C / min, for example, 0.2°C / min, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 4°C / min or 5°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In the present invention, the oxidative curing can increase the molecular weight of the raw material and improve the softening temperature, so that the precursor is not melted during deep oxidation, thereby facilitating the acquisition of a highly cross-linked oxidative precursor.
[0041] As a preferred technical solution of the present invention, the inert atmosphere in step (2) includes any one of helium, neon or argon, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of helium and neon, a combination of neon and argon, a combination of helium, neon and argon, etc.
[0042] Preferably, the pyrolysis in step (2) is carried out in a pyrolysis furnace to remove volatiles from the oxidative precursor.
[0043] Preferably, the pyrolysis temperature in step (2) is 300-900°C, for example, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C or 900°C, but is not limited to the listed values. Other values not listed within this numerical range are also applicable. The time is 0.5-3h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h or 3h, but is not limited to the listed values. Other values not listed within this numerical range are also applicable.
[0044] Preferably, the heating rate of the pyrolysis in step (2) is 0.5 to 10°C / min, for example, 0.5°C / min, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 8°C / min or 10°C / min, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0045] Preferably, after the pyrolysis in step (2), the product is transferred to a carbonization furnace for high-temperature carbonization, preferably in a constant temperature zone of the carbonization furnace.
[0046] In the present invention, the pyrolysis product can be directly transferred to the carbonization furnace without cooling, or can be transferred after cooling.
[0047] Preferably, the temperature of the high-temperature carbonization in step (2) is 1300-1500°C, for example, 1300°C, 1320°C, 1350°C, 1380°C, 1400°C, 1420°C, 1450°C, 1480°C or 1500°C, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0048] Preferably, the heating rate of the high-temperature carbonization in step (2) is 0.5 to 3°C / min, for example, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0049] Preferably, the high-temperature carbonization time in step (2) is 1 to 5 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0050] Preferably, after the high-temperature carbonization in step (2), an inert atmosphere is continuously introduced while the furnace is cooled.
[0051] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0052] (1) The carbon source precursor is first crushed and screened, and the carbon source precursor includes any one of coal tar pitch, petroleum pitch, coal or heavy carbon, or a combination of at least two of them. The crushing includes crushing and grinding in sequence. After crushing, the raw material particles are first dried and then ground to obtain raw material particles. The particle size of the raw material particles selected by screening is 3 to 20 μm. After drying, the raw material particles are pickled and deashed. The acid used for pickling and deashing includes hydrochloric acid and / or hydrofluoric acid. The carbon source precursor is first mixed with hydrochloric acid with a mass fraction of 10 to 37% and then stirred and washed. The solid-liquid ratio of the carbon source precursor to the hydrochloric acid is 1 g: (2 to 10) mL. After standing, the carbon source precursor is washed with water, filtered, and dried to obtain a first pickling raw material; the first pickling raw material is mixed with hydrofluoric acid with a mass fraction of 25 to 40% and then stirred and washed. The solid-liquid ratio of the first pickling raw material to the hydrofluoric acid is 1 g: (1 to 10) mL. After standing, the carbon source precursor is washed with water, filtered, and dried to obtain a second pickling raw material;
[0053] Then, oxidative curing and deep oxidation are sequentially performed under an oxygen-containing atmosphere, wherein the oxygen concentration in the oxygen-containing atmosphere is 10-100%, the concentration of the oxygen-containing atmosphere is independently selected during oxidative curing and deep oxidation, the oxidative curing and deep oxidation are performed consecutively, and after the oxidative curing is completed, the temperature is continuously raised for deep oxidation, the oxidative curing temperature is lower than the softening point temperature of the carbon source precursor or the temperature corresponding to the maximum weight when thermogravimetry is selected, the oxidative curing temperature is 70-320° C., the time is 1-5 h, and the heating rate is 0.2-5° C. / min; the deep oxidation temperature is 120-360° C., the time is 1-5 h, and the heating rate is 0.2-5° C. / min, to obtain an oxidized precursor;
[0054] (2) The oxidative precursor obtained in step (1) is pyrolyzed in an inert atmosphere to remove volatiles, wherein the inert atmosphere includes any one of helium, neon or argon or a combination of at least two of them, the pyrolysis temperature is 300-900°C, the heating rate is 0.5-10°C / min, and the time is 0.5-3h, and then high-temperature carbonization is performed, the high-temperature carbonization temperature is 1300-1500°C, the heating rate is 0.5-3°C / min, and the time is 1-5h. After the high-temperature carbonization, the inert atmosphere is continuously introduced and the temperature is lowered as the furnace cools to obtain a hard carbon negative electrode material.
[0055] In a second aspect, the present invention provides a hard carbon negative electrode material obtained by the above preparation method.
[0056] As a preferred technical solution of the present invention, the particle size of the hard carbon negative electrode material is 3 to 10 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0057] Preferably, the specific surface area of the hard carbon negative electrode material is 3 to 8 m 2 / g, for example 3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g or 8m 2 / g, etc., but are not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0058] Preferably, the interlayer spacing of the crystal plane (002) of the hard carbon negative electrode material is 0.37 to 0.39 nm, for example, 0.37 nm, 0.372 nm, 0.375 nm, 0.377 nm, 0.38 nm, 0.382 nm, 0.385 nm, 0.388 nm or 0.39 nm, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0059] In a third aspect, the present invention provides a use of the hard carbon negative electrode material described above, wherein the hard carbon negative electrode material is used in the preparation of a sodium ion battery as a component of a negative electrode sheet in a sodium ion battery.
[0060] In the present invention, when the hard carbon negative electrode material is used in a sodium ion battery, it is necessary to first prepare a negative electrode sheet and then assemble it into a battery; the preparation process of the negative electrode sheet includes the steps of grinding, slurrying, and coating;
[0061] In the grinding and pulping process, the negative electrode active material, the conductive agent, and the binder are mixed and ground in proportion, bonded, and stirred to prepare the pulp. The specific process parameters are: the conductive agent is conductive carbon black SP, the binder is carboxymethyl cellulose CMC and styrene-butadiene rubber SBR, the mass ratio of the negative electrode active material, SP, CMC, and SBR is 90:4:2:4, the single cup homogenizer is stirred for 27 minutes at a speed of 1950 r / min, and the degassing is carried out for 3 minutes at a speed of 2150 r / min;
[0062] In the coating process, the coating thickness is 100 μm and the surface density is controlled at 2-3 mg / cm 2 After the electrode is dried, it is rolled and directly cut into pieces and weighed.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] (1) The method of the present invention is to perform oxidation curing and deep oxidation on the carbon source precursor respectively. The former can increase the molecular weight of the raw material and increase its melting temperature, thereby avoiding the problems of slow mass transfer rate and uneven oxidation caused by melting when directly oxidizing at a higher temperature. Then, deep oxidation cross-linking is performed to obtain an oxidized precursor with a high degree of oxidation and a complex cross-linked structure. After pyrolysis to remove volatiles and then combined with high-temperature carbonization treatment, the disorder and interplanar spacing of the carbon layer are increased, thereby improving the sodium storage performance of the negative electrode material, and the capacity and rate performance are excellent;
[0065] (2) The method of the present invention is easy to operate, has low raw material and process costs, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] Figure 1 is the XRD pattern of the hard carbon negative electrode material provided in Example 3 of the present invention and Comparative Example 2;
[0067] Figure 2 is a Raman spectrum of the hard carbon negative electrode material provided in Example 3 of the present invention and Comparative Example 2;
[0068] Figure 3a is a TEM image of the hard carbon negative electrode material provided in Example 3 of the present invention;
[0069] Figure 3b This is a TEM image of the hard carbon negative electrode material provided in Comparative Example 2 of the present invention;
[0070] Figure 4 is a charge and discharge curve diagram of a sodium ion battery assembled with the hard carbon negative electrode material provided in Example 3 of the present invention;
[0071] Figure 5 This is a rate curve of a sodium ion battery assembled with the hard carbon negative electrode material provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0072] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0073] The following are typical but non-limiting examples of the present invention:
[0074] Example 1:
[0075] This embodiment provides a method for preparing a hard carbon negative electrode material, the preparation method comprising the following steps:
[0076] (1) The carbon source precursor is first crushed and sieved. The carbon source precursor is coal tar pitch. The crushing includes crushing and grinding in sequence. After crushing, it is first dried and then ground to obtain raw material particles. The average particle size of the raw material particles selected by screening is 10 μm. After drying, it is acid washed and deashed. The acid washing and deashing are first washed with hydrochloric acid and then with hydrofluoric acid. The carbon source precursor is first mixed with hydrochloric acid with a mass fraction of 18% and then stirred and washed at a speed of 100 r / min for 12 hours. The solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1g:10mL. After standing for 2 hours, it is washed with water until there is no Cl - , filtered and dried at 105 ° C for 12 hours to obtain a first pickling raw material; the first pickling raw material was mixed with 30% hydrofluoric acid by mass and then stirred and washed at a speed of 100 r / min for 24 hours, the solid-liquid ratio of the first pickling raw material to hydrofluoric acid was 1g:7.5mL, and then washed with water until there was no F - , filtered and dried at 105°C for 12 hours to obtain a second acid-washed raw material;
[0077] Then, oxidative curing and deep oxidation are carried out in sequence under an air atmosphere, and the oxidative curing and deep oxidation are carried out consecutively. After the oxidative curing is completed, the temperature is continued to be raised for deep oxidation. The oxidative curing temperature is 270°C, which is 10°C lower than the softening point of coal tar pitch, the heating rate is 0.5°C / min, and the time is 5 hours. The deep oxidation temperature is 330°C, the heating rate is 0.5°C / min, and the time is 2 hours to obtain an oxidized precursor.
[0078] (2) The oxidative precursor obtained in step (1) is pyrolyzed in an argon atmosphere to remove volatiles, wherein the pyrolysis temperature is 700°C, the heating rate is 2°C / min, and the time is 3 hours, and then high-temperature carbonization is performed, wherein the high-temperature carbonization temperature is 1400°C, the heating rate is 1°C / min, and the time is 5 hours. After the high-temperature carbonization, argon is continuously introduced and the furnace is cooled to obtain a hard carbon negative electrode material.
[0079] Example 2:
[0080] This embodiment provides a method for preparing a hard carbon negative electrode material, the preparation method comprising the following steps:
[0081] (1) The carbon source precursor is first crushed and sieved. The carbon source precursor is petroleum asphalt. The crushing includes crushing and grinding in sequence. After crushing, it is first dried and then ground to obtain raw material particles. The average particle size of the raw material particles selected by screening is 5 μm. After drying, it is acid washed and deashed. The acid washing and deashing are first washed with hydrochloric acid and then with hydrofluoric acid. The carbon source precursor is first mixed with hydrochloric acid with a mass fraction of 10% and then stirred and washed at a speed of 90 r / min for 14 hours. The solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1g:8mL. After standing for 1 hour, it is washed with water until there is no Cl - , filtered and dried at 100 ° C for 15 hours to obtain a first pickling raw material; the first pickling raw material was mixed with 25% hydrofluoric acid by mass and washed at a speed of 90r / min for 26 hours, the solid-liquid ratio of the first pickling raw material to hydrofluoric acid was 1g:10mL, and then washed with water until there was no F - , filtered and dried at 100°C for 15h to obtain a second pickling raw material;
[0082] Then, oxidative curing and deep oxidation are carried out in sequence under an air atmosphere, the oxidative curing and deep oxidation are carried out consecutively, and after the oxidative curing is completed, the temperature is continued to be raised for deep oxidation, the oxidative curing temperature is 70°C, which is 10°C lower than the softening point of petroleum asphalt, the heating rate is 1°C / min, and the time is 4 hours, and the deep oxidation temperature is 125°C, the heating rate is 1°C / min, and the time is 3 hours to obtain an oxidized precursor;
[0083] (2) The oxidative precursor obtained in step (1) is pyrolyzed in an argon atmosphere to remove volatiles, the pyrolysis temperature is 400°C, the heating rate is 0.5°C / min, and the time is 2 hours, and then high-temperature carbonization is performed, the high-temperature carbonization temperature is 1300°C, the heating rate is 0.5°C / min, and the time is 4 hours. After the high-temperature carbonization, argon is continuously introduced and the furnace is cooled to obtain a hard carbon negative electrode material.
[0084] Example 3:
[0085] This embodiment provides a method for preparing a hard carbon negative electrode material, the preparation method comprising the following steps:
[0086] (1) The carbon source precursor is first crushed and sieved. The carbon source precursor is bituminous coal. The crushing includes crushing and grinding in sequence. After crushing, it is first dried and then ground to obtain raw material particles. The average particle size of the raw material particles selected by screening is 15 μm. After drying, it is acid washed and deashed. The acid washing and deashing are first washed with hydrochloric acid and then with hydrofluoric acid. The carbon source precursor is first mixed with hydrochloric acid with a mass fraction of 37% and then stirred and washed at a speed of 110 r / min for 10 hours. The solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1g:2mL. After standing for 3 hours, it is washed with water until there is no Cl - , filtered and dried at 120 ° C for 10 hours to obtain a first pickling raw material; the first pickling raw material was mixed with 40% hydrofluoric acid by mass and stirred at a speed of 110r / min for 22 hours, the solid-liquid ratio of the first pickling raw material to hydrofluoric acid was 1g:2mL, and then washed with water until there was no F - , filtered and dried at 120°C for 10 hours to obtain a second pickling raw material;
[0087] Then, oxidation curing and deep oxidation are carried out in sequence under air atmosphere, the oxidation curing and deep oxidation are carried out consecutively, and after the oxidation curing is completed, the temperature is continued to be raised for deep oxidation, the oxidation curing temperature is 310° C., the heating rate is 1.5° C. / min, and the time is 5 h, and the deep oxidation temperature is 355° C., the time is 5 h, and the heating rate is 1.5° C. / min, to obtain an oxidation precursor;
[0088] (2) The oxidative precursor obtained in step (1) is pyrolyzed in an argon atmosphere to remove volatiles, wherein the pyrolysis temperature is 800°C, the heating rate is 4°C / min, and the time is 2 hours, and then high-temperature carbonization is performed, wherein the high-temperature carbonization temperature is 1400°C, the heating rate is 1°C / min, and the time is 5 hours. After the high-temperature carbonization, argon is continuously introduced and the furnace is cooled to obtain a hard carbon negative electrode material.
[0089] Example 4:
[0090] This embodiment provides a method for preparing a hard carbon negative electrode material, the preparation method comprising the following steps:
[0091] (1) The carbon source precursor is first crushed and screened. The carbon source precursor is coal liquefaction residue. The crushing includes crushing and grinding in sequence. After crushing, it is first dried and then ground to obtain raw material particles. The average particle size of the raw material particles selected by screening is 12 μm. After drying, it is acid washed and deashed. The acid washing and deashing are first washed with hydrochloric acid and then with hydrofluoric acid. The carbon source precursor is first mixed with hydrochloric acid with a mass fraction of 30% and then stirred and washed at a speed of 120 r / min for 12 hours. The solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1g:4mL. After standing for 2 hours, it is washed with water until there is no Cl - , filtered and dried at 110 ° C for 12 hours to obtain a first pickling raw material; the first pickling raw material was mixed with 35% hydrofluoric acid by mass and stirred at a speed of 120r / min for 20 hours, the solid-liquid ratio of the first pickling raw material to hydrofluoric acid was 1g:5mL, and then washed with water until there was no F - , filtered and dried at 110°C for 12 hours to obtain a second acid-washed raw material;
[0092] Then, oxidative curing and deep oxidation were carried out in sequence under air atmosphere, the oxidative curing and deep oxidation were carried out consecutively, and after the oxidative curing was completed, the temperature was continued to be raised for deep oxidation, the oxidative curing temperature was 270° C., the heating rate was 4° C. / min, and the time was 4 h, and the deep oxidation temperature was 340° C., the heating rate was 2.5° C. / min, and the time was 5 h, to obtain an oxidized precursor;
[0093] (2) The oxidative precursor obtained in step (1) is pyrolyzed in a neon atmosphere to remove volatiles, wherein the pyrolysis temperature is 900°C, the heating rate is 8°C / min, and the time is 1 hour, and then high-temperature carbonization is performed, wherein the high-temperature carbonization temperature is 1350°C, the heating rate is 1.5°C / min, and the time is 3 hours. After the high-temperature carbonization, neon gas is continuously introduced and the furnace is cooled to obtain a hard carbon negative electrode material.
[0094] Example 5:
[0095] This embodiment provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that: the atmosphere conditions for oxidative curing and deep oxidation in step (1) are a mixture of oxygen and argon, with an oxygen concentration of 40%; the temperature for oxidative curing is 292°C, and the temperature for deep oxidation is 320°C.
[0096] Example 6:
[0097] This embodiment provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that: the atmosphere conditions for oxidative curing and deep oxidation in step (1) are a mixture of oxygen and argon, with an oxygen concentration of 80%; the temperature for oxidative curing is 273°C, and the temperature for deep oxidation is 320°C.
[0098] Example 7:
[0099] This embodiment provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that the temperature of the high-temperature carbonization in step (2) is 1500° C. and the heating rate is 3° C. / min.
[0100] Example 8:
[0101] This embodiment provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that: the pyrolysis temperature in step (2) is 600°C, the heating rate is 3°C / min, and the time is 3h.
[0102] Comparative Example 1:
[0103] This comparative example provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 1, except that: in step (1), no oxidation curing is performed, and deep oxidation is performed directly, and the time is the total time of the original oxidation curing and deep oxidation, which is 7 hours.
[0104] Comparative Example 2:
[0105] This comparative example provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that: in step (1), no oxidation curing is performed, and deep oxidation is performed directly, and the time is the total time of the original oxidation curing and deep oxidation, which is 10 hours.
[0106] Comparative Example 3:
[0107] This comparative example provides a method for preparing a hard carbon negative electrode material. The preparation method refers to the method in Example 3, except that the heating rate of the high-temperature carbonization in step (2) is 5°C / min.
[0108] The structural parameters of the hard carbon negative electrode materials prepared in Examples 1-8 and Comparative Examples 1-3 are shown in Table 1, wherein the XRD patterns of the hard carbon negative electrode materials in Example 3 and Comparative Example 2 are shown in Table 1. Figure 1 As shown, the Raman spectrum is Figure 2 As shown, the TEM image of the hard carbon negative electrode material in Example 3 is as follows Figure 3a As shown, the TEM image of the hard carbon negative electrode material in Comparative Example 2 is as follows Figure 3b shown.
[0109] Table 1
[0110]
[0111]
[0112] d in Table 1 002 refers to the interlayer spacing of the (002) crystal plane of the hard carbon negative electrode material, Lc refers to the thickness of the radial carbon microcrystal, La refers to the length of the carbon microcrystal, I D / I G It refers to the ratio of amorphous carbon to graphite phase carbon in carbon microcrystals, describing the degree of defects in carbon microcrystals.
[0113] As shown in Table 1, the interlayer spacing of the (002) crystal plane in the examples is above 0.37 nm, and I D / I G All are above 2.0, which is significantly higher than the data in the comparative example; Figure 1 From the XRD diagram, it can be seen that the characteristic peak intensity corresponding to the (002) crystal plane in Example 3 is relatively small, indicating that its graphitization degree is low. Figure 2 As can be seen from the Raman spectrum in the graph, the ratio of the peak areas representing amorphous carbon and graphitized carbon is higher in Example 3; Figure 3a and Figure 3b From the TEM image, we can see the interplanar spacing of the (002) crystal plane, and it can be concluded that the interplanar spacing in Example 3 is greater than that in Comparative Example 2; it can be seen that the hard carbon negative electrode material prepared in the embodiment of the present invention has a wide interplanar spacing and a high degree of amorphism, which helps to improve the battery performance.
[0114] The hard carbon negative electrode materials prepared in the above Examples 1-8 and Comparative Examples 1-3 are used to prepare negative electrode sheets, which are then used in the assembly of sodium ion batteries; wherein the preparation process of the negative electrode sheets includes the steps of grinding, slurrying, and coating; specifically, the hard carbon negative electrode material, SP, CMC, and SBR are ground in a mass ratio of 90:4:2:4, and slurried by bonding and magnetic stirring. The process parameters are: stirring for 27 minutes in a single cup homogenizer at a speed of 1950 r / min, degassing for 3 minutes at a speed of 2150 r / min; in the coating process, the coating thickness is 100 μm, and the surface density is controlled at 2 to 3 mg / cm 2 , the negative electrode sheet is rolled after drying and directly cut into pieces and weighed;
[0115] The positive electrode of the sodium ion battery is sodium, the electrolyte is 1 mol NaFP6 dissolved in ethylene carbonate EC and dimethyl carbonate DMC in a volume ratio of 1:1, the separator is glass fiber GF / D, and the electrochemical test is performed after assembly. The conditions of the electrochemical test are: standing time 7h, discharge at 0.1C, charge at 0.1C, and cut-off voltages of 5mV and 2V respectively; the test environment is: temperature 25±1°C, humidity 40% RH; the results of the electrochemical test are shown in Table 2, wherein the charge and discharge curves of the sodium ion battery assembled with the hard carbon negative electrode material in Example 3 are shown in Table 2. Figure 4 As shown, the rate curve is Figure 5 shown.
[0116] Table 2
[0117]
[0118]
[0119] As shown in Table 2, when the sodium ion batteries assembled with the hard carbon negative electrode materials in the examples were subjected to electrochemical tests, the first charge specific capacity at a current density of 0.1C reached 275 mAh g -1 Above, the first coulombic efficiency can reach more than 85%; specifically taking Example 3 as an example, Figure 4 and Figure 5 It can be seen that during the first three charge and discharge processes, at a current density of 0.1C, the charge capacity remained basically unchanged. As the rate increased, the charge capacity remained above 200mAh / g, indicating that the material has good rate performance and is conducive to improving the fast charging capability of the battery.
[0120] Comparative Examples 1 and 2 are both operations without oxidative curing. Compared with the corresponding embodiments, their degree of oxidation and cross-linking are low, which results in a decrease in sodium storage capacity and rate performance; in Comparative Example 3, the heating rate is too high during high-temperature carbonization, and the surface melting reaction easily prevents the internal reaction from continuing, resulting in uneven reaction during the carbonization process and inability to fully carbonize the interior, thereby reducing the sodium storage performance.
[0121] From the above embodiments and comparative examples, it can be seen that the method of the present invention performs oxidation curing and deep oxidation on the carbon source precursor respectively. The former can increase the molecular weight of the raw material and improve its melting temperature, avoiding the problems of slow mass transfer rate and uneven oxidation caused by melting when directly oxidizing at a higher temperature. Deep oxidation and cross-linking are then performed to obtain an oxidized precursor with a high degree of oxidation and a complex cross-linked structure. After thermal decomposition to remove volatiles and combined with high-temperature carbonization treatment, the disorder and interplanar spacing of the carbon layer are improved, thereby improving the sodium storage performance of the negative electrode material, and the capacity and rate performance are excellent. The method is simple to operate, has low raw material and process costs, and has a wide range of applications.
[0122] The applicant declares that the present invention uses the above-described embodiments to illustrate the detailed methods of the present invention. However, the present invention is not limited to the above-described detailed methods, and does not necessarily rely on the above-described detailed methods for implementation. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions for the methods of the present invention, additions of auxiliary steps, and selections of specific methods, etc., fall within the scope of protection and disclosure of the present invention.
Claims
1. A method for preparing a hard carbon negative electrode material, characterized in that: The preparation method comprises the following steps: (1) acid-washing and deashing the carbon source precursor, and then sequentially performing oxidation curing and deep oxidation in an oxygen-containing atmosphere, wherein the temperature of the oxidation curing is lower than the temperature of the deep oxidation, to obtain an oxidized precursor; (2) The oxidized precursor obtained in step (1) is subjected to pyrolysis and high-temperature carbonization in an inert atmosphere to obtain a hard carbon negative electrode material.
2. The preparation method according to claim 1, characterized in that: The carbon source precursor in step (1) includes any one of coal tar pitch, petroleum pitch, coal or heavy carbon, or a combination of at least two thereof; Preferably, the carbon source precursor in step (1) is first crushed and sieved to obtain raw material particles; Preferably, the pulverization includes crushing and grinding in sequence, and the crushing is first dried and then ground; Preferably, the particle size of the raw material particles selected by screening is 3 to 20 μm; Preferably, the sieved raw material particles are dried and then acid washed and deashed.
3. The preparation method according to claim 1 or 2, characterized in that: The acid solution used for pickling and deashing in step (1) includes hydrochloric acid and / or hydrofluoric acid, preferably, hydrochloric acid is used for washing first, and then hydrofluoric acid is used for washing; Preferably, the carbon source precursor is mixed with hydrochloric acid, stirred and washed, left to stand, washed with water, filtered, and dried to obtain a first acid-washed raw material; Preferably, the solid-liquid ratio of the carbon source precursor to hydrochloric acid is 1 g: (2-10) mL; Preferably, the mass fraction of the hydrochloric acid is 10 to 37%; Preferably, the first pickling raw material is mixed with hydrofluoric acid, stirred and washed, left to stand, washed with water, filtered, and dried to obtain a second pickling raw material; Preferably, the solid-to-liquid ratio of the first pickling raw material to hydrofluoric acid is 1 g: (1-10) mL; Preferably, the mass fraction of the hydrofluoric acid is 25-40%.
4. The preparation method according to any one of claims 1 to 3, characterized in that The concentration of oxygen in the oxygen-containing atmosphere in step (1) is 10 to 100%; Preferably, the concentration of the oxygen-containing atmosphere in step (1) is independently selected during oxidative curing and deep oxidation, preferably the same concentration; Preferably, the oxidative curing and deep oxidation in step (1) are both carried out in a tube furnace, preferably in a constant temperature zone of the tube furnace; Preferably, the oxidative curing and deep oxidation in step (1) are carried out consecutively, and after the oxidative curing is completed, the temperature is continued to be raised for deep oxidation.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The temperature of the oxidative curing in step (1) is lower than the softening point of the carbon source precursor or the temperature corresponding to the maximum weight when thermogravimetry is selected; Preferably, the temperature of the oxidative curing in step (1) is 70 to 320°C, the time is 1 to 5 hours, and the heating rate is 0.2 to 5°C / min; Preferably, the temperature of the deep oxidation in step (1) is 120-360° C., the time is 1-5 h, and the heating rate is 0.2-5° C. / min.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The inert atmosphere in step (2) comprises any one of helium, neon or argon, or a combination of at least two of them; Preferably, the pyrolysis in step (2) is carried out in a pyrolysis furnace to remove volatiles from the oxidative precursor; Preferably, the pyrolysis temperature in step (2) is 300-900°C and the time is 0.5-3h; Preferably, the heating rate of the pyrolysis in step (2) is 0.5 to 10°C / min; Preferably, after the pyrolysis in step (2), the product is transferred to a carbonization furnace for high-temperature carbonization, preferably in a constant temperature zone of the carbonization furnace; Preferably, the temperature of the high temperature carbonization in step (2) is 1300-1500°C; Preferably, the heating rate of the high temperature carbonization in step (2) is 0.5-3°C / min; Preferably, the high temperature carbonization time in step (2) is 1 to 5 hours; Preferably, after the high-temperature carbonization in step (2), an inert atmosphere is continuously introduced to cool the furnace.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) The carbon source precursor is first crushed and screened, wherein the carbon source precursor includes any one of coal tar pitch, petroleum pitch, coal or heavy carbon or a combination of at least two thereof, wherein the crushing includes crushing and grinding in sequence, wherein the crushing is first dried and then ground to obtain raw material particles, wherein the particle size of the raw material particles selected by the screening is 3 to 20 μm, and then the raw material particles are acid washed and deashed after drying, wherein the acid solution used for the acid washing and deashing includes hydrochloric acid and / or hydrofluoric acid, wherein the carbon source precursor is first mixed with hydrochloric acid having a mass fraction of 10 to 37%, and then stirred and washed, wherein the solid-liquid ratio of the carbon source precursor to the hydrochloric acid is 1 g: (2 to 10) mL, and then the carbon source precursor is allowed to stand and then washed with water, filtered and dried to obtain a first acid washed raw material; wherein the first acid washed raw material is mixed with hydrofluoric acid having a mass fraction of 25 to 40%, and then stirred and washed, wherein the solid-liquid ratio of the first acid washed raw material to the hydrofluoric acid is 1 g: (1 to 10) mL, and then the carbon source precursor is allowed to stand and then washed with water, filtered and dried to obtain a second acid washed raw material; Then, oxidation curing and deep oxidation are carried out in sequence under an oxygen-containing atmosphere, wherein the concentration of oxygen in the oxygen-containing atmosphere is 10-100%, and the concentration of the oxygen-containing atmosphere is independently selected during oxidation curing and deep oxidation, and the oxidation curing and deep oxidation are carried out consecutively. After the oxidation curing is completed, the temperature is continuously raised for deep oxidation, and the oxidation curing temperature is lower than the softening point temperature of the carbon source precursor or the temperature corresponding to the maximum weight when thermogravimetry is selected, and the oxidation curing temperature is 70-320° C., the time is 1-5 hours, and the heating rate is 0.2-5° C. / min; the deep oxidation temperature is 120-360° C., the time is 1-5 hours, and the heating rate is 0.2-5° C. / min, to obtain an oxidation precursor; (2) The oxidative precursor obtained in step (1) is pyrolyzed in an inert atmosphere to remove volatiles, wherein the inert atmosphere includes any one of helium, neon or argon or a combination of at least two of them, the pyrolysis temperature is 300-900°C, the heating rate is 0.5-10°C / min, and the time is 0.5-3h, followed by high-temperature carbonization, wherein the high-temperature carbonization temperature is 1300-1500°C, the heating rate is 0.5-3°C / min, and the time is 1-5h, and after the high-temperature carbonization, the inert atmosphere is continuously introduced and the temperature is lowered as the furnace cools to obtain a hard carbon negative electrode material.
8. The hard carbon negative electrode material obtained according to the preparation method according to any one of claims 1 to 7.
9. The hard carbon negative electrode material according to claim 8, characterized in that: The particle size of the hard carbon negative electrode material is 3 to 10 μm; Preferably, the specific surface area of the hard carbon negative electrode material is 3 to 8 m 2 / g; Preferably, the interlayer spacing of the (002) crystal plane of the hard carbon negative electrode material is 0.37-0.39 nm.
10. Use of the hard carbon negative electrode material according to claim 8 or 9, characterized in that: The hard carbon negative electrode material is used for the preparation of sodium ion batteries and serves as a component of the negative electrode plate in the sodium ion batteries.
Citation Information
Patent Citations
Oxidized asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of oxidized asphalt-based hard carbon negative electrode material
CN115991467A
Sodium-ion battery negative electrode active material and preparation method and application thereof
CN116239099A
High-power asphalt-based sodium ion battery carbon negative electrode material as well as preparation method and application thereof
CN117125694A
Sodium-ion battery hard carbon negative electrode material and preparation method thereof
CN117163936A
Asphalt derived carbon sodium ion battery negative electrode material and preparation method and application thereof
CN117342541A
Cited By
Lignite-based hard carbon negative electrode material, preparation method and application thereof
CN120328524A