Intrinsic graphene preform with adjustable X-band electromagnetic performance and preparation method thereof

The intrinsic graphene preforms were prepared by liquid phase peeling method and rotary evaporation method. Combined with the use of gel agent and pore-forming agent, the limitations of graphene oxide preforms in microstructure and electromagnetic function regulation were solved, and the X-band was achieved The preparation of intrinsic graphene preforms with adjustable electromagnetic properties is suitable for reinforcement of composite materials.

CN118954493AActive Publication Date: 2024-11-15NORTHWESTERN POLYTECHNICAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411034027.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The raw materials of graphene preforms in the existing composite materials are graphene oxide, which leads to limited regulation of microstructure and electromagnetic function during assembly, and it is difficult to completely remove oxygen-containing functional groups and defects, resulting in conductive performance lag behind intrinsic performance.

Method used

The intrinsic graphene water-based suspension was prepared by liquid phase peeling method, and a high-concentration dispersion was prepared by rotary evaporation method. The gel agent and pore-forming agent were added for ultrasonic treatment, and shearing and freeze-drying were carried out to form a low content. The intrinsic graphene preform with oxygen functional groups and low Raman defects achieves the regulation of its microstructure and electromagnetic properties.

Benefits of technology

Overcoming the limitations of graphene oxide preforms in microstructure and electromagnetic function regulation, an intrinsic graphene preform with X-band electromagnetic properties with good forming effect and mechanical strength was prepared, which is suitable for the enhancement of metal-based composite materials. body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954493A_ABST
    Figure CN118954493A_ABST
Patent Text Reader

Abstract

The invention discloses an intrinsic graphene preform with adjustable X-band electromagnetic performance and a preparation method thereof, and belongs to the technical field of functional materials. The preparation method comprises the following steps: preparing an intrinsic graphene water-based suspension; preparing an intrinsic graphene dispersion liquid; adding a gelling agent and a pore forming agent, and performing ultrasonic treatment to obtain an intrinsic graphene mixed solution; performing shearing treatment to obtain an intrinsic graphene aqueous solution; adding a foam stabilizer into the intrinsic graphene aqueous solution, and performing ultrasonic treatment to obtain intrinsic graphene hydrogel; freezing the intrinsic graphene hydrogel to obtain intrinsic graphene hydrogel ice crystals, and then drying the intrinsic graphene hydrogel ice crystals to obtain an intrinsic graphene preform. The intrinsic graphene preform prepared by the preparation method is used for coping with external complex electromagnetic environment changes and developing an X-band highly-integrated homogeneous self-adaptive electromagnetic composite material, and can overcome the defects when graphene oxide is used as the preform; and according to the preparation method, the problems of poor forming effect and high preparation difficulty of the existing intrinsic graphene preform are further solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and in particular relates to an intrinsic graphene preform with adjustable X-band electromagnetic properties and a preparation method thereof. Background Art

[0002] With the rapid development of 5G communications, satellite phones, radio transmitters and radar detectors, the development of highly integrated homogeneous adaptive electromagnetic materials in the X-band is an effective way to cope with changes in the complex external electromagnetic environment. Graphene, with its unique nanoscale, excellent mechanical properties, large specific surface area, good microwave absorption function and excellent electrothermal transmission characteristics, has broad application prospects in the fields of electromagnetic materials and supercapacitors. Among them, graphene preforms, as an important form of graphene assembly, have the characteristics of high porosity, excellent electrical conductivity and microstructure designability. When used as reinforcements in metal-based composites, the microstructure controllability and electromagnetic performance controllability of graphene preforms can be effectively utilized to ensure that the prepared metal-based composites can autonomously control the impedance matching between the material and the air and meet the requirements of adjustable electromagnetic performance, which puts higher requirements on the microstructure and electromagnetic properties of graphene preforms.

[0003] For example, the Chinese patent with publication number CN113148996A discloses that a three-dimensional reduced graphene oxide porous absorbing material is prepared by mixing a graphene oxide aqueous solution, a reducing agent and an antifreeze agent, magnetically stirring, ultrasonically dispersing, freezing, thawing at room temperature, and freezing and thawing. By controlling the pore size and volume of the absorbing material, effective absorption of 6 to 18 GHz can be achieved. The raw materials of the three-dimensional porous graphene preforms currently prepared are all graphene oxide. The more oxygen-containing functional groups on its surface cause it to spontaneously form a honeycomb network structure when assembled into a three-dimensional preform, and its microstructure regulation and electromagnetic wave response regulation are limited. In addition, the more oxygen-containing functional groups and defects on the surface of graphene oxide cannot be completely removed after the reduction treatment, so that its conductive properties lag behind its intrinsic properties. Summary of the invention

[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide an intrinsic graphene preform with adjustable X-band electromagnetic properties and a preparation method thereof, so as to solve the technical problem that the raw materials of graphene preforms in current composite materials are all graphene oxide, and the large number of oxygen-containing functional groups limit the regulation of microstructure and electromagnetic functionality when assembled into a three-dimensional preform, and the large number of oxygen-containing functional groups and defects cannot be completely removed after reduction treatment, so that the conductivity and functionality still lag behind the intrinsic performance.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties, comprising the following steps:

[0007] S1: taking raw graphite powder, and subjecting it to multiple ultrasonic exfoliations using a liquid phase exfoliation method to obtain an intrinsic graphene water-based suspension; taking the upper clear liquid from the intrinsic graphene water-based suspension, and preparing an intrinsic graphene dispersion using a rotary evaporation method;

[0008] S2: adding a gelling agent and a pore-forming agent to the intrinsic graphene dispersion, and performing ultrasonic treatment to obtain an intrinsic graphene mixed solution;

[0009] S3: performing shearing treatment on the intrinsic graphene mixed solution to obtain an intrinsic graphene aqueous solution;

[0010] S4: adding a foam stabilizer to the intrinsic graphene aqueous solution and performing ultrasonic treatment to obtain an intrinsic graphene hydrogel;

[0011] S5: freezing the intrinsic graphene hydrogel to obtain intrinsic graphene hydrogel ice crystals, and drying the intrinsic graphene hydrogel ice crystals to obtain an intrinsic graphene preform.

[0012] In one embodiment, in S1, the concentration of the intrinsic graphene dispersion is 5 to 15 mg / ml.

[0013] In one embodiment, in S1, the mass ratio of graphene in the supernatant of the intrinsic graphene water-based suspension to the raw graphite powder is 1:8-14.

[0014] In one embodiment, in S1, the intrinsic graphene in the intrinsic graphene dispersion has a sheet size of 5 to 15 μm, a thickness of 0.5 to 1.5 nm, and a Raman defect degree I D / I G The value is 0.1~0.4;

[0015] The viscosity of the supernatant is 1.30-1.52 cP, and the surface tension is 65-68 mN / m.

[0016] In one embodiment, in S2, the gelling agent is polyvinyl alcohol or sodium carboxymethyl cellulose, and the mass ratio of intrinsic graphene to gelling agent in the intrinsic graphene mixed solution is 4 to 16:1.

[0017] In one embodiment, in S2, the pore former is sodium dodecyl sulfate or polystyrene, and the mass ratio of the intrinsic graphene to the pore former in the intrinsic graphene mixed solution is 1:0-8.

[0018] In one embodiment, in S3, the rotation speed of the shearing treatment is 800 to 2600 rpm, and the time of the shearing treatment is 2 to 22 min.

[0019] In one embodiment, in S4, the foam stabilizer is one or more of riboflavin sodium phosphate and sodium dodecylbenzene sulfonate, and the mass ratio of the intrinsic graphene in the intrinsic graphene hydrogel to the foam stabilizer is 15 to 40:1.

[0020] In one embodiment, in S5, the freezing temperature is -180 to -20°C, the freezing time is 10 to 720 minutes, and the drying time is 36 to 48 hours.

[0021] The present invention also provides an intrinsic graphene preform prepared by adopting the method for preparing the intrinsic graphene preform with adjustable X-band electromagnetic properties.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The invention provides a method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties. Graphite powder is subjected to liquid phase exfoliation to prepare an intrinsic graphene water-based suspension, a rotary evaporation method is adopted to prepare a high-concentration intrinsic graphene dispersion, an intrinsic graphene dispersion with low Raman defect degree, less oxygen-containing functional groups and lower viscosity is used as a raw material, a gelling agent and a pore-forming agent are added to perform ultrasonic treatment to obtain an intrinsic graphene mixed solution, the gelling agent is added to solve the problem of weak gelation of intrinsic graphene and increase the viscosity of the intrinsic graphene dispersion, and since the intrinsic graphene has less oxygen-containing functional groups, it can only form a cross-linked structure by combining the carboxyl group in the gelling agent with the hydroxyl group in the water, which is helpful for the subsequent forming of the intrinsic graphene preform; the pore-forming agent is added to solve the problem of easy agglomeration of intrinsic graphene and can also adjust the microscopic pore size structure of the intrinsic graphene preform; then the intrinsic graphene mixed solution is subjected to high-speed The intrinsic graphene aqueous solution is obtained by shearing treatment. The high-speed shearing is to stir the intrinsic graphene mixed solution to form bubbles, form a pore structure between the stacked intrinsic graphene sheets, and the intrinsic graphene sheets are evenly and tightly arranged around the bubbles, which is conducive to the construction of the three-dimensional network structure of the intrinsic graphene preform and the uniform dispersion of the sheets; then a foam stabilizer is added for ultrasonic treatment to obtain an intrinsic graphene hydrogel. The foam stabilizer is added to stabilize the generated bubbles so that the bubbles are evenly distributed and to ensure the uniform distribution of the intrinsic graphene sheets. The hydrophilic group of the foam stabilizer is combined with water, and the hydrophobic group is combined with the intrinsic graphene sheets, which can simultaneously achieve the effects of stabilizing the bubbles and uniformly dispersing the intrinsic graphene sheets; finally, the intrinsic graphene hydrogel is freeze-dried to obtain an intrinsic graphene preform. The intrinsic graphene preform with adjustable X-band electromagnetic properties prepared by the invention can be used as a reinforcement of a metal-based composite material.

[0024] On the other hand, the present invention provides an intrinsic graphene preform with adjustable X-band electromagnetic properties obtained by the above-mentioned preparation method, which can be used as a raw material for graphene preforms in response to changes in complex external electromagnetic environments and in the development of highly integrated homogeneous adaptive electromagnetic composite materials in the X-band. In addition to the advantages of the intrinsic graphene preform having fewer defects and oxygen-containing functional groups, designable microstructure, adjustable electromagnetic properties and low preparation cost, more importantly, the intrinsic graphene preform obtained by the above-mentioned preparation method has the advantages of good forming effect and certain mechanical strength, which solves the problems of poor forming effect and great preparation difficulty of existing intrinsic graphene preforms. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The middle figures (a), (b), (c) and (d) are scanning electron microscope images of the intrinsic graphene preforms prepared in Examples 1, 3, 4 and 6 of the present invention, respectively. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0027] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0028] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0029] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0030] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0031] The intrinsic graphene preform proposed in the present invention has the advantages of designable microstructure, adjustable electromagnetic properties and low preparation cost. On the one hand, the lower defects and fewer oxygen-containing functional groups of intrinsic graphene give it the advantage of microstructural designability, so that it has rich adjustable properties in the field of electromagnetic functions; on the other hand, it does not need to be heat treated later, and the preparation cost is low. However, the intrinsic graphene preform has the problems of poor forming effect and great difficulty in preparation, which limit the application of intrinsic graphene in microstructure and electromagnetic property regulation. Therefore, it is necessary to explore a method for preparing an intrinsic graphene preform with certain mechanical strength and adjustable electromagnetic properties.

[0032] The present invention provides an intrinsic graphene preform with adjustable electromagnetic properties in the X-band and a preparation method thereof, the purpose of which is to cope with changes in complex external electromagnetic environments and develop highly integrated homogeneous adaptive electromagnetic composite materials in the X-band, solve the problem that the raw materials of graphene preforms in the current composite materials are all graphene oxide, and the more oxygen-containing functional groups limit the regulation of microstructure and electromagnetic functionality when assembled into a three-dimensional preform, and the more oxygen-containing functional groups and defects cannot be completely removed after reduction treatment, so that its conductivity and functionality still lag behind the intrinsic performance. The intrinsic graphene preform has the advantages of fewer defects and oxygen-containing functional groups, designable microstructure, adjustable electromagnetic properties and low preparation cost. However, compared with graphene oxide, the intrinsic graphene preform has the problems of poor forming effect and great preparation difficulty, and provides a method for preparing an intrinsic graphene preform with adjustable electromagnetic properties in the X-band.

[0033] On the one hand, the present invention provides a method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties, comprising the following steps:

[0034] 1) taking raw graphite powder, and using liquid phase exfoliation method to obtain a black intrinsic graphene water-based suspension after multiple ultrasonic exfoliation; taking the upper clear liquid, and using rotary evaporation method to prepare an intrinsic graphene dispersion with a concentration of 5 to 15 mg / ml;

[0035] The mass ratio of graphene to raw graphite powder in the black intrinsic graphene supernatant is 1:8-14; the sheet size of intrinsic graphene is 5-15 μm, the thickness is 0.5-1.5 nm, and the Raman defect degree is I D / I G The value is 0.1-0.4, the viscosity of the intrinsic graphene supernatant is 1.30-1.52 cP, and the surface tension is 65-68 mN / m.

[0036] 2) adding a gelling agent and a pore-forming agent to the intrinsic graphene dispersion prepared in step 1), and performing ultrasonic treatment to obtain an intrinsic graphene mixed solution;

[0037] By adding a gelling agent, the viscosity of the intrinsic graphene dispersion is increased, a cross-linked structure is formed, and the intrinsic graphene preform is formed. By adding a pore-forming agent, the problem of easy agglomeration of intrinsic graphene sheets is solved and the microscopic pore structure of the graphene preform is regulated. The gelling agent is polyvinyl alcohol or sodium carboxymethyl cellulose, and the mass ratio of intrinsic graphene to gelling agent in the intrinsic graphene mixed solution is 4 to 16:1. The gelling agent is added here to solve the problem of weak gelation of intrinsic graphene and increase the viscosity of the intrinsic graphene dispersion. Since intrinsic graphene contains fewer oxygen functional groups, This can only form a cross-linked structure with the help of the carboxyl group in the gelling agent and the hydroxyl group in the water, which is helpful for the subsequent formation of the intrinsic graphene preform; the pore-forming agent is sodium dodecyl sulfate or polystyrene, and the mass ratio of the intrinsic graphene to the pore-forming agent in the intrinsic graphene mixed solution is 1:0-8. Since the intrinsic graphene surface has low defects and fewer oxygen-containing functional groups, the larger van der Waals force interaction between the intrinsic graphene sheets makes the sheets tend to stack together. The pore-forming agent is added here to solve the problem of easy agglomeration of intrinsic graphene, and can also regulate the microscopic pore size structure of the graphene preform;

[0038] The ultrasonic power is 40 to 200 W, and the ultrasonic time is 3 to 20 min;

[0039] 3) subjecting the intrinsic graphene mixed solution obtained in step 2) to high-speed shearing treatment to obtain an intrinsic graphene aqueous solution;

[0040] The shearing speed is 800-2600 rpm, and the shearing time is 2-22 min. The shearing action is to stir the intrinsic graphene mixed solution to form bubbles, form a pore structure between the stacked intrinsic graphene sheets, and the intrinsic graphene sheets are evenly and tightly arranged around the bubbles, which is conducive to the construction of the three-dimensional network structure of the intrinsic graphene preform and the uniform dispersion of the sheets;

[0041] 4) adding a foam stabilizer to the intrinsic graphene aqueous solution prepared in step 3), and performing ultrasonic treatment to obtain an intrinsic graphene hydrogel;

[0042] The foam stabilizer is one or more of riboflavin sodium phosphate and sodium dodecylbenzene sulfonate. The mass ratio of intrinsic graphene to the foam stabilizer in the intrinsic graphene hydrogel is 15 to 40:1. The foam stabilizer is added here to stabilize the bubbles generated in step 3) so that the bubbles are evenly distributed, and to ensure that the intrinsic graphene sheets are evenly distributed. The hydrophilic group of the foam stabilizer is combined with water, and the hydrophobic group is combined with the intrinsic graphene sheet, which can simultaneously achieve the effect of stabilizing the bubbles and uniformly dispersing the intrinsic graphene sheets. In short, the effect of uniformly stabilizing the bubbles and uniformly dispersing the intrinsic graphene sheets is achieved by adding the foam stabilizer;

[0043] The ultrasonic power is 40 to 200 W, and the ultrasonic time is 3 to 15 minutes;

[0044] 5) placing the intrinsic graphene hydrogel prepared in step 4) in a freezing mold, placing the mold in a freezing container for freezing to obtain intrinsic graphene hydrogel ice crystals, and drying the intrinsic graphene hydrogel ice crystals to obtain an intrinsic graphene preform;

[0045] The freezing temperature is -180 to -20°C, the freezing time is 10 to 720 minutes, and the drying time is 36 to 48 hours.

[0046] The intrinsic graphene preform prepared by the above method can be used as a reinforcement of metal-based composite materials, and the electromagnetic properties of the metal-based composite materials can be regulated by introducing preforms with different electromagnetic properties into the matrix.

[0047] The present invention overcomes the problem of limited regulation of the microstructure and electromagnetic properties of existing three-dimensional reduced graphene oxide, and utilizes the advantage that intrinsic graphene has fewer oxygen-containing functional groups and thus has an adjustable microstructure of a three-dimensional preform, to prepare an intrinsic graphene preform with certain mechanical strength and adjustable microstructure and electromagnetic properties. By adjusting the ratio of intrinsic graphene to pore-forming agent and the freezing temperature of intrinsic graphene hydrogel, effective regulation of multiple properties such as wave transmission, electromagnetic shielding and wave absorption can be achieved. The raw material used in the preparation of the above-mentioned preform is intrinsic graphene. Compared with graphene oxide, intrinsic graphene has fewer structural defects and lower viscosity of aqueous solution. D / I G The value is 0.1 to 0.4, and the viscosity is 1.30 to 1.52 cP. Although the intrinsic graphene solution has the disadvantages of weak gelation and easy stacking of the sheets, the present invention can effectively solve this problem by adding a gelling agent and a foaming agent. The prepared intrinsic graphene preform has a certain mechanical strength. When the compression strain is 50%, the compression stress is 3 to 50 kPa, and it can be used as a reinforcement for metal-based composite materials. In addition, the present invention adds a foam stabilizer after the bubbles are generated by high-speed shearing. On the one hand, it is to stabilize the bubbles and make the bubbles evenly distributed. On the other hand, the foam stabilizer also plays the role of a surfactant, which is helpful for the uniform dispersion of the intrinsic graphene sheets.

[0048] Another aspect of the present invention provides an intrinsic graphene preform prepared by the above method, and by changing the ratio of intrinsic graphene to pore-forming agent and the freezing temperature of intrinsic graphene hydrogel, an intrinsic graphene preform with certain mechanical properties and adjustable electromagnetic properties is obtained, and the density of the material is 0.03-0.07 g / cm 3, porosity is 90-96%. The material can achieve effective regulation of transmittance of 92%-98%, electromagnetic shielding effectiveness of ~45dB, and electromagnetic wave absorption minimum reflection loss between -50.7 and -10.6dB in the 8.2-12.4GHz band, which is significantly different from the three-dimensional structure of reduced graphene oxide in terms of single electromagnetic performance regulation.

[0049] The principle of the present invention is as follows: since intrinsic graphene and graphene oxide have significant differences in defect degree, number of oxygen-containing functional groups, dispersion viscosity, hydrophilicity, etc., graphene oxide has the characteristics of strong gelation and spontaneous formation of a three-dimensional honeycomb network structure, which is completely different from the characteristics of intrinsic graphene weak gelation and tendency of flakes to stack. Therefore, the preparation of the intrinsic graphene preform by the present invention is different from the existing preparation method of graphene oxide aerogel, breaking the conventional thinking. Specifically, graphite powder is subjected to liquid phase exfoliation to prepare an intrinsic graphene water-based suspension, a high-concentration intrinsic graphene dispersion is prepared by rotary evaporation, an intrinsic graphene dispersion with a low Raman defect degree, a small number of oxygen-containing functional groups, and a low viscosity is used as a raw material, a gelling agent and a pore-forming agent are added for ultrasonic treatment to obtain an intrinsic graphene mixed solution, the gelling agent is added to solve the problem of weak gelation of intrinsic graphene and to increase the viscosity of the intrinsic graphene dispersion, since the intrinsic graphene contains few oxygen-containing functional groups, it can only form a cross-linked structure with the help of the carboxyl group in the gelling agent and the hydroxyl group in the water, which is helpful for the subsequent formation of the intrinsic graphene preform; the pore-forming agent is added to solve the problem of easy agglomeration of intrinsic graphene, and at the same time, the microscopic pore structure of the intrinsic graphene preform can be adjusted; then the intrinsic graphene mixed solution is subjected to high-speed shear treatment to obtain an intrinsic graphene water-soluble The method comprises the following steps: stirring the intrinsic graphene mixed solution at a high speed to form bubbles, forming a pore structure between the stacked intrinsic graphene sheets, and evenly and closely arranging the intrinsic graphene sheets around the bubbles, which is conducive to the construction of the three-dimensional network structure of the intrinsic graphene preform and the uniform dispersion of the sheets; then adding a foam stabilizer for ultrasonic treatment to obtain an intrinsic graphene hydrogel, the foam stabilizer is added to stabilize the generated bubbles so that the bubbles are evenly distributed, and also to ensure the uniform distribution of the intrinsic graphene sheets, the hydrophilic group of the foam stabilizer is combined with the water, and the hydrophobic group is combined with the intrinsic graphene sheets, which can simultaneously achieve the effects of stabilizing the bubbles and uniformly dispersing the intrinsic graphene sheets; finally, the intrinsic graphene hydrogel is freeze-dried to obtain an intrinsic graphene preform, and the intrinsic graphene preform with adjustable X-band electromagnetic properties prepared by the present invention can be used as a reinforcement of metal-based composite materials.

[0050] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0051] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0052] The present invention relates to a method for preparing an intrinsic graphene water-based suspension by liquid phase exfoliation and preparing a high-concentration intrinsic graphene dispersion by rotary evaporation, and typical steps thereof are exemplified as follows:

[0053] (1) adding 30 mg / ml of graphite powder and 1.5 mg / ml of riboflavin sodium phosphate to deionized water and stirring at 300 W for 4.5 h to obtain a black intrinsic graphene water-based suspension;

[0054] (2) After standing for 48 hours, the supernatant was taken and a 5-15 mg / ml intrinsic graphene dispersion was prepared by rotary evaporation at a temperature of 60° C. for 4 hours.

[0055] The above is a known technology.

[0056] Example 1

[0057] This embodiment provides a method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties, and the specific steps are as follows:

[0058] Step 1: Take 5 mg / ml intrinsic graphene dispersion, add polyvinyl alcohol and sodium dodecyl sulfate to the intrinsic graphene dispersion according to the mass ratio of intrinsic graphene to polyvinyl alcohol of 4:1 and the mass ratio of intrinsic graphene to sodium dodecyl sulfate of 1:0, and treat with an ultrasonic power of 40 W for 20 minutes to obtain an intrinsic graphene mixed solution;

[0059] Step 2: The intrinsic graphene mixed solution is sheared at a rotation speed of 800 rpm for 22 minutes to obtain an intrinsic graphene aqueous solution;

[0060] Step 3: adding riboflavin sodium phosphate to the intrinsic graphene aqueous solution in a mass ratio of intrinsic graphene to riboflavin sodium phosphate of 15:1, and subjecting to 40W ultrasonic treatment for 15 minutes to obtain an intrinsic graphene hydrogel;

[0061] Step 4: Place the intrinsic graphene hydrogel in a freezing mold, place the mold in a freezing container and freeze at -20°C for 720 minutes to obtain intrinsic graphene hydrogel ice crystals, and dry the intrinsic graphene hydrogel ice crystals for 36 hours to obtain an intrinsic graphene preform. The prepared intrinsic graphene preform has wave-transmitting properties, and the X-band electromagnetic wave transmittance is 98%.

[0062] Example 2

[0063] The difference from Example 1 is that the concentration of the intrinsic graphene dispersion in step 1 is 10 mg / ml, and the mass ratio of intrinsic graphene to polyvinyl alcohol is 10:1. In step 4, the mold is placed in a freezing container and frozen at -100°C for 360 minutes. The prepared intrinsic graphene preform has wave-transmitting properties, and the X-band electromagnetic wave transmittance is ~97%.

[0064] Example 3

[0065] The difference from Example 1 is that the concentration of the intrinsic graphene dispersion taken in step 1 is 15 mg / ml, and the mass ratio of intrinsic graphene to polyvinyl alcohol is 12:1. In step 4, the mold is placed in a freezing container and frozen at -180°C for 10 minutes. The prepared intrinsic graphene preform has wave-transmitting properties, and the X-band electromagnetic wave transmittance is ~92%.

[0066] Example 4

[0067] This embodiment provides a method for preparing an intrinsic graphene preform with adjustable electromagnetic properties, and the specific steps are as follows:

[0068] Step 1: Take 10 mg / ml intrinsic graphene dispersion, add sodium carboxymethyl cellulose and sodium dodecyl sulfate to the intrinsic graphene dispersion according to the mass ratio of intrinsic graphene to sodium carboxymethyl cellulose of 10:1 and the mass ratio of intrinsic graphene to sodium dodecyl sulfate of 1:3, and treat with an ultrasonic power of 120 W for 12 minutes to obtain an intrinsic graphene mixed solution;

[0069] Step 2: The intrinsic graphene mixed solution is sheared at a rotation speed of 1700 rpm for 12 minutes to obtain an intrinsic graphene aqueous solution;

[0070] Step 3: adding riboflavin sodium phosphate to the intrinsic graphene aqueous solution in a mass ratio of intrinsic graphene to riboflavin sodium phosphate of 27:1, and subjecting to 120W ultrasonic treatment for 9 minutes to obtain an intrinsic graphene hydrogel;

[0071] Step 4: Place the intrinsic graphene hydrogel in a freezing mold, place the mold in a freezing container and freeze at -180°C for 10 minutes to obtain intrinsic graphene hydrogel ice crystals, and dry the intrinsic graphene hydrogel ice crystals for 42 hours to obtain an intrinsic graphene preform. The prepared intrinsic graphene preform has wave absorbing properties, and the minimum reflection loss of X-band electromagnetic wave absorption is -50.7dB.

[0072] Example 5

[0073] The difference from Example 4 is that the mass ratio of intrinsic graphene to sodium dodecyl sulfate in step 1 is 1:5. In step 4, the mold is placed in a freezing container and frozen at -20°C for 720 minutes. The prepared intrinsic graphene preform has wave absorbing performance, and the minimum reflection loss of X-band electromagnetic wave absorption is -10.6dB.

[0074] Example 6

[0075] This embodiment provides a method for preparing an intrinsic graphene preform with adjustable electromagnetic properties, and the specific steps are as follows:

[0076] Step 1: Take 10 mg / ml intrinsic graphene dispersion, add sodium carboxymethyl cellulose and polystyrene to the intrinsic graphene dispersion according to the mass ratio of intrinsic graphene to sodium carboxymethyl cellulose of 16:1 and the mass ratio of intrinsic graphene to polystyrene of 1:8, and treat with an ultrasonic power of 200 W for 3 minutes to obtain an intrinsic graphene mixed solution;

[0077] Step 2: The intrinsic graphene mixed solution is sheared at a rotation speed of 2600 rpm for 2 minutes to obtain an intrinsic graphene aqueous solution;

[0078] Step 3: adding riboflavin sodium phosphate to the intrinsic graphene aqueous solution in a mass ratio of intrinsic graphene to sodium dodecylbenzene sulfonate of 40:1, and subjecting the mixture to ultrasonic treatment at 200 W for 3 min to obtain an intrinsic graphene hydrogel;

[0079] Step 4: Place the intrinsic graphene hydrogel in a freezing mold, place the mold in a freezing container and freeze at -20°C for 720 minutes to obtain intrinsic graphene hydrogel ice crystals, and dry the intrinsic graphene hydrogel ice crystals for 48 hours to obtain an intrinsic graphene preform. The prepared intrinsic graphene preform has electromagnetic shielding performance, with an X-band total shielding effectiveness of 45.34 dB, a reflection effectiveness of 5.88 dB, and a reflection effectiveness of 39.46 dB.

[0080] Example 7

[0081] The difference from Example 6 is that in step 4, the mold is placed in a freezing container and frozen at -180°C for 10 minutes. The prepared intrinsic graphene preform has electromagnetic shielding performance, with an X-band total shielding effectiveness of 44.95 dB, a reflection effectiveness of 4.40 dB, and a reflection effectiveness of 40.55 dB.

[0082] like Figure 1 As shown, the intrinsic graphene preform prepared in Example 1 shown in Figure (a) shows that the intrinsic graphene without adding a pore-forming agent and frozen at a higher temperature tends to stack to form large sheets due to the interaction of interlayer van der Waals forces, and does not form a connected network structure, which is helpful for constructing an intrinsic graphene wave-transmitting material. The intrinsic graphene preform prepared in Example 3 shown in Figure (b) shows that the intrinsic graphene without adding a pore-forming agent can be oriented by increasing the intrinsic graphene content and reducing the freezing temperature of the intrinsic graphene hydrogel. The intrinsic graphene preform prepared in Example 4 shown in Figure (c) shows that the addition of a small amount of pore-forming agent can make the pores of the oriented arrangement of the intrinsic graphene more uniform and regular, and wrinkles appear on the surface of the large sheet formed. The oriented uniform pores can regulate the impedance matching between the material and the free space, which is helpful for forming an intrinsic graphene wave-absorbing material. From the intrinsic graphene preform prepared in Example 6 shown in Figure (d), it can be seen that the intrinsic graphene sheets with increased content of pore-forming agent and frozen at a higher temperature can be assembled into a three-dimensional network structure, which is helpful to form an intrinsic graphene electromagnetic shielding material.

[0083] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties, characterized in that: The following steps are involved: S1: taking raw graphite powder, and subjecting it to multiple ultrasonic exfoliations using a liquid phase exfoliation method to obtain an intrinsic graphene water-based suspension; taking the upper clear liquid from the intrinsic graphene water-based suspension, and preparing an intrinsic graphene dispersion using a rotary evaporation method; S2: adding a gelling agent and a pore-forming agent to the intrinsic graphene dispersion, and performing ultrasonic treatment to obtain an intrinsic graphene mixed solution; S3: performing shearing treatment on the intrinsic graphene mixed solution to obtain an intrinsic graphene aqueous solution; S4: adding a foam stabilizer to the intrinsic graphene aqueous solution and performing ultrasonic treatment to obtain an intrinsic graphene hydrogel; S5: freezing the intrinsic graphene hydrogel to obtain intrinsic graphene hydrogel ice crystals, and drying the intrinsic graphene hydrogel ice crystals to obtain an intrinsic graphene preform.

2. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S1, the concentration of the intrinsic graphene dispersion is 5 to 15 mg / ml.

3. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S1, the mass ratio of graphene in the supernatant of the intrinsic graphene water-based suspension to the raw graphite powder is 1:8-14.

4. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S1, the intrinsic graphene in the intrinsic graphene dispersion has a sheet size of 5 to 15 μm, a thickness of 0.5 to 1.5 nm, and a Raman defect degree I D / I G The value is 0.1~0.4; The viscosity of the supernatant is 1.30-1.52 cP, and the surface tension is 65-68 mN / m.

5. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S2, the gelling agent is polyvinyl alcohol or sodium carboxymethyl cellulose, and the mass ratio of intrinsic graphene to gelling agent in the intrinsic graphene mixed solution is 4 to 16:

1.

6. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S2, the pore-forming agent is sodium dodecyl sulfate or polystyrene, and the mass ratio of the intrinsic graphene to the pore-forming agent in the intrinsic graphene mixed solution is 1:0-8.

7. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S3, the rotation speed of the shearing treatment is 800 to 2600 rpm, and the time of the shearing treatment is 2 to 22 minutes.

8. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S4, the foam stabilizer is one or more of riboflavin sodium phosphate and sodium dodecylbenzene sulfonate, and the mass ratio of the intrinsic graphene in the intrinsic graphene hydrogel to the foam stabilizer is 15 to 40:

1.

9. The method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to claim 1, characterized in that: In S5, the freezing temperature is -180 to -20°C, the freezing time is 10 to 720 minutes, and the drying time is 36 to 48 hours.

10. An intrinsic graphene preform obtained by the method for preparing an intrinsic graphene preform with adjustable X-band electromagnetic properties according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Three-dimensional graphene foam as well as preparation method and application thereof

    CN106698409A

  • Method for peeling graphene under assistance of cellulose in conjugate base system

    CN109665519A

  • High-temperature post-treatment-free graphene ink for flexible device printing and preparation method of high-temperature post-treatment-free graphene ink

    CN114891399A

  • Method for preparing graphene by utilizing graphite negative electrode of recycled waste lithium ion battery

    CN115959654A

  • Method for preparing perforated graphene on large scale based on liquid phase stripping

    CN117509628A