Regenerated positive electrode precursor and preparation method thereof, regenerated positive electrode material and preparation method thereof, lithium ion battery and electric equipment
By mixing the used lithium-ion battery positive electrode material with boric acid solution and lithium source, a regenerated positive electrode precursor is formed and sintered, the problems of high energy consumption and poor performance in the recycling of lithium-ion battery positive electrode material are solved, and high efficiency and low cost regeneration is achieved Preparation of positive electrode materials improves electrochemical performance.
Patent Information
- Application Number
- CN202410996045.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium-ion battery cathode material recycling technology has problems such as high energy consumption, high cost, unfriendly environment and poor repair performance. Especially when the surface phase change structure hinders the embedding of lithium ions, it is difficult to achieve the performance of fresh cathode materials.
Use the use of used positive electrode material and boric acid solution, add lithium source and chelating agent, and then form a regenerated positive electrode precursor through heating and drying, and then obtain the regenerated positive electrode material through sintering. The reaction of boric acid and the surface spinel structure removes obstacles, and enhances the embeddedness of lithium. properties and material properties.
It realizes the preparation of recycled positive electrode materials with simple operation, low cost and low energy consumption, and improves the structural stability and electrochemical performance of the materials, which is suitable for large-scale promotion and application.
Smart Images

Figure CN118954527A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of recycling of waste battery materials, and in particular to a regenerated positive electrode precursor and a preparation method thereof, a regenerated positive electrode material and a preparation method thereof, a lithium-ion battery and electrical equipment. Background Art
[0002] Lithium-ion batteries are widely used in 3C electronic products, new energy vehicles, portable electronic products and energy storage equipment due to their advantages such as high energy density, long cycle stability and low self-discharge. However, after 3 to 5 years of use, the capacity of lithium-ion batteries will gradually decrease due to factors such as material failure, electrolyte decomposition and violent side reactions, which will not meet product demand and will inevitably produce a large number of waste lithium-ion batteries. The positive electrode material of lithium-ion batteries is one of the key electrode materials that determine the electrochemical performance of batteries and has great recycling value. On the one hand, the positive electrode materials of waste lithium-ion batteries contain many metals, such as a large amount of valuable metals such as lithium, cobalt and nickel in the ternary positive electrode. On the other hand, the transition metals and organic electrolytes contained in the positive electrode materials of waste lithium-ion batteries will cause environmental pollution. Therefore, the reasonable recycling and reuse of them can not only save resources, but also reduce environmental pollution. If improperly handled, it will not only cause the loss of valuable metals, but also cause serious pollution to water and soil and cause great harm to human health.
[0003] At present, there are mainly the following technologies for recycling the positive electrode materials of waste lithium-ion batteries:
[0004] The first is to smelt the positive electrode material at high temperature through pyrometallurgy and purify it through physical and chemical transformation. This process will produce a large amount of toxic gas and high energy consumption.
[0005] The second method is to use traditional hydrometallurgical technology to leach the valuable metal ions in the positive electrode material and then precipitate and separate them to prepare the precursor raw materials. This technology has problems such as long process flow, high cost, and large reagent consumption.
[0006] The third is physical repair and regeneration technology. For some positive electrodes that lack lithium, lithium is supplemented and repaired, and the crystals are reshaped and regenerated into secondary positive electrode materials. This method is simple in process, low in cost, and environmentally friendly. It has been a hot topic of concern in industry and academia in recent years. However, after a long cycle, the surface structure of the positive electrode material undergoes a phase change, from a layered structure with better lithium ion deintercalation to a spinel structure with fewer ion pathways, and finally to a rock salt structure without lithium ion pathways. Therefore, during the repair process, the coating layer of the surface phase change will hinder the embedding of lithium ions, resulting in the inability of lithium ions to enter the lithium-deficient vacancies in the bulk phase of the material during the high-temperature repair process, resulting in the performance of the repaired positive electrode material being difficult to reach the level of a fresh positive electrode. Summary of the invention
[0007] The purpose of the present application is to provide a regenerated positive electrode precursor and a preparation method thereof, a regenerated positive electrode material and a preparation method thereof, a lithium-ion battery and an electrical device to solve the above-mentioned problems.
[0008] To achieve the above objectives, this application adopts the following technical solutions:
[0009] A method for preparing a regenerated positive electrode precursor comprises: mixing waste positive electrode materials with a boric acid solution, and then adding a lithium source to obtain a first mixed solution; mixing the first mixed solution with a chelating agent to obtain a second mixed solution; and heating and drying the second mixed solution to obtain the regenerated positive electrode precursor.
[0010] According to an embodiment of the present application, the waste positive electrode material includes any one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium cobalt oxide;
[0011] And / or, the concentration of the boric acid solution is 0.02-1 mol / L;
[0012] And / or, the waste positive electrode material and the boric acid solution are mixed for 30 to 60 minutes;
[0013] And / or, the solid-to-liquid ratio of the waste positive electrode material to the boric acid solution is 1:(1-5) g / mL;
[0014] And / or, the waste positive electrode material is prepared by the following method: disassembling and separating waste lithium-ion batteries to obtain positive electrode sheets, calcining the positive electrode sheets at a temperature of 450 to 550° C. for 1 to 4 hours, and the waste positive electrode material falls off from the current collector to obtain the waste positive electrode material.
[0015] According to an embodiment of the present application, the lithium source includes a lithium salt or a hydrate of the lithium salt, and the lithium salt includes any one of LiOH, Li2CO3, LiNO3, CH3COOLi, LiCl, and Li2SO4;
[0016] And / or, the ratio of the sum of the molar amount of lithium in the lithium source and the molar amount of lithium in the waste positive electrode material to the molar amount of non-lithium metal in the waste positive electrode material is (1.03-1.08):1.
[0017] According to an embodiment of the present application, the molar amount of the chelating agent is 1.0 to 1.3 times the sum of the molar amount of the non-lithium metal in the waste positive electrode material and the molar amount of lithium in the lithium source;
[0018] And / or, the chelating agent includes at least one of citric acid, maleic acid, malic acid, and oxalic acid.
[0019] According to an embodiment of the present application, preparing the regenerated positive electrode precursor includes: firstly heating the second mixed liquid to form a gel, and then drying the gel to obtain the regenerated positive electrode precursor;
[0020] And / or, the forming of gel comprises: stirring the second mixed solution at a temperature of 60 to 80° C. for 1 to 4 hours to form a gel;
[0021] And / or, the temperature of the drying process is 110-130°C.
[0022] And / or, the drying process is performed for 9 to 11 hours.
[0023] The present application also provides a regenerated positive electrode precursor, which is prepared by the preparation method of the regenerated positive electrode precursor described above.
[0024] The present application also provides a method for preparing a regenerated positive electrode material, comprising: sintering the regenerated positive electrode precursor mentioned above to obtain the regenerated positive electrode material.
[0025] According to an embodiment of the present application, the sintering is performed in an oxygen-containing atmosphere;
[0026] And / or, the sintering includes: heating the regenerated positive electrode precursor to 450-550° C. at a rate of 5-10° C. / min, and keeping the temperature for 4-6 hours, and then heating the regenerated positive electrode precursor to 800-950° C. at a rate of 5-10° C. / min, and keeping the temperature for 10-15 hours;
[0027] And / or, after the sintering is completed, the temperature is lowered to 180-220° C. at a rate of 5-10° C. / min, and then cooled to room temperature to obtain the regenerated positive electrode material.
[0028] The present application also provides a regenerated positive electrode material, which is prepared by the preparation method of the regenerated positive electrode material described above.
[0029] The present application also provides a lithium-ion battery, which includes the regenerated positive electrode material described above.
[0030] The present application also provides an electrical device, which includes the lithium-ion battery described above.
[0031] Compared with the prior art, the beneficial effects of this application include:
[0032] The present application adds boric acid to the preparation method of the regenerated positive electrode precursor, and utilizes the reaction of boric acid with the spinel structure and rock salt structure of the surface layer of the waste positive electrode material that undergo phase change, so that the spinel structure and rock salt structure of the surface layer of the waste positive electrode material that undergo phase change can be removed, so that the supplemented lithium can more easily enter the lithium vacancies of the waste positive electrode material. At the same time, the boron in the boric acid can also be doped into the waste positive electrode material to improve the performance of the regenerated positive electrode precursor or the regenerated positive electrode material. Moreover, the method of the present application also has the advantages of simple operation, low production cost, low energy consumption, environmental friendliness, and reusability after regeneration, which is conducive to large-scale promotion and application.
[0033] The regenerated positive electrode material of the present application is obtained by sintering a regenerated positive electrode precursor, and the regenerated positive electrode material has excellent performance.
[0034] The lithium-ion battery and electrical equipment of the present application have excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0036] Figure 1 is a scanning electron microscope image of the waste positive electrode material NCM523 in Example 1;
[0037] Figure 2 is a scanning electron microscope image of the regenerated positive electrode material R-NCM523 in Example 1;
[0038] Figure 3 This is a scanning electron microscope image of the regenerated positive electrode material R-NCM523 in comparative example 1. DETAILED DESCRIPTION
[0039] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:
[0040] A method for preparing a regenerated positive electrode precursor comprises: mixing waste positive electrode materials with a boric acid solution, then adding a lithium source to obtain a first mixed solution; mixing the first mixed solution with a chelating agent to obtain a second mixed solution; and heating and drying the second mixed solution to obtain the regenerated positive electrode precursor.
[0041] Therefore, boric acid can react with the spinel and rock salt structures that undergo phase change on the surface of the waste positive electrode material, and then remove the structure that undergoes phase change on the surface of the waste positive electrode material, making it easier for the supplemented lithium to enter the lithium vacancies in the bulk phase of the material, making the structure of the recycled material more complete. At the same time, boron can also be doped into the positive electrode material to improve the structural stability and the performance of the regenerated positive electrode precursor.
[0042] According to the embodiment of the present application, the waste positive electrode material includes lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide (LiNi 0.8 Co 0.15 Al 0.05 O2), lithium cobalt oxide (LiCoO2); further, lithium nickel cobalt manganese oxide includes LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2 or LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0043] And / or, the concentration of the boric acid solution is 0.02-1 mol / L; for example, the concentration of the boric acid solution can be 0.02 mol / L, 0.05 mol / L, 0.10 mol / L, 0.15 mol / L, 0.20 mol / L, 0.25 mol / L, 0.30 mol / L, 0.35 mol / L, 0.40 mol / L, 0.45 mol / L, 0.50 mol / L, 0.55 mol / L, 0.60 mol / L, 0.65 mol / L, 0.70 mol / L, 0.75 mol / L, 0.80 mol / L, 0.85 mol / L, 0.90 mol / L, 0.95 mol / L, 1 mol / L; at this concentration, boric acid can completely react with the structure of the phase change on the surface of the waste positive electrode material, which is beneficial for the supplemented lithium to enter the lithium vacancies in the waste positive electrode material and is beneficial for improving the performance of the regenerated positive electrode material. If the concentration of boric acid is too low, the spinel or rock salt structure on the surface of the waste positive electrode material cannot be completely removed. The unremoved spinel or rock salt structure will hinder the embedding of lithium ions, and the performance improvement of the regenerated positive electrode material will be small. If the concentration of boric acid is too high, the reaction will be too violent.
[0044] And / or, the time for mixing the waste positive electrode material with the boric acid solution is 30 to 60 minutes; for example, the time for mixing the waste positive electrode material with the boric acid solution can be 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, and 60 minutes. Thus, within the above time range, it can be ensured that the structure that undergoes phase change on the surface of the waste positive electrode material is completely removed, which is conducive to improving the performance of the regenerated positive electrode material.
[0045] And / or, the solid-liquid ratio of the waste positive electrode material to the boric acid solution is 1:(1-5) g / mL. For example, the solid-liquid ratio of the waste positive electrode material to the boric acid solution can be 1:1 g / mL, 1:2 g / mL, 1:3 g / mL, 1:4 g / mL, 1:5 g / mL. In this way, the spinel and rock salt structure that undergo phase change on the surface of the waste positive electrode material can be completely removed, which is beneficial to the improvement of the performance of the regenerated positive electrode material.
[0046] According to an embodiment of the present application, the waste positive electrode material is prepared by the following method: disassembling and separating waste lithium-ion batteries to obtain positive electrode sheets, calcining the positive electrode sheets at a temperature of 450 to 550°C (e.g., 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C) for 1 to 4 hours (e.g., 1 hour, 2 hours, 3 hours, 4 hours), and the waste positive electrode material falls off from the current collector to obtain the waste positive electrode material. By calcining under the above conditions, the binder can be decomposed and inactivated, the waste positive electrode material on the current collector can be fallen off, and the separation between the waste positive electrode material and the current collector can be achieved.
[0047] According to an embodiment of the present application, the lithium source includes a lithium salt or a hydrate of the lithium salt, and the lithium salt includes any one of LiOH, Li2CO3, LiNO3, CH3COOLi, LiCl, and Li2SO4; since the loss of lithium in the waste positive electrode material is the main reason for the decline in the capacity of the positive electrode material, by adding a lithium source, the missing lithium can be replenished back to the positive electrode material and the material structure can be repaired, which is beneficial to improving the electrochemical performance of the regenerated positive electrode material. For example, the hydrate of the lithium salt can be LiOH·H2O.
[0048] And / or, the ratio of the sum of the molar amount of lithium in the lithium source and the molar amount of lithium in the waste positive electrode material to the molar amount of non-lithium metal in the waste positive electrode material is (1.03-1.08):1. For example, the ratio of the sum of the molar amount of lithium in the lithium source and the molar amount of lithium in the waste positive electrode material to the molar amount of non-lithium metal in the waste positive electrode material can be 1.03:1, 1.04:1, 1.05:1, 1.06:1, 1.07:1, 1.08:1. In this way, it can be ensured that the regenerated positive electrode material can obtain excellent electrochemical performance. If the content of the lithium source is too little, that is, the amount of lithium supplementation is insufficient, the lithium vacancies in the positive electrode material are not fully supplemented, resulting in a small improvement in the performance of the regenerated positive electrode material; if the content of the lithium source is too much, the performance of the positive electrode material will be reduced.
[0049] According to an embodiment of the present application, the molar amount of the chelating agent is 1.0 to 1.3 times the sum of the molar amount of the non-lithium metal in the waste positive electrode material and the molar amount of lithium in the lithium source. For example, the molar amount of citric acid is 1, 1.1, 1.2 or 1.3 times the sum of the molar amount of the non-lithium metal in the waste positive electrode material and the molar amount of lithium in the lithium source.
[0050] According to an embodiment of the present application, the chelating agent includes at least one of citric acid, maleic acid, malic acid, and oxalic acid.
[0051] According to an embodiment of the present application, preparing the regenerated positive electrode precursor includes: firstly heating the second mixed liquid to form a gel, and then drying the gel to obtain the regenerated positive electrode precursor;
[0052] According to an embodiment of the present application, the forming of the gel comprises: stirring the second mixed solution at a temperature of 60 to 80° C. (e.g., 60° C., 65° C., 70° C., 75° C., 80° C.) for 1 to 4 hours (e.g., 1 hour, 2 hours, 3 hours, or 4 hours) to form a gel;
[0053] And / or, the temperature of the drying process is 110-130°C; for example, the temperature of the drying process can be 110°C, 115°C, 120°C, 125°C, 130°C;
[0054] And / or, the drying time is 9 to 11 hours, for example, the drying time can be 9 hours, 10 hours, or 11 hours.
[0055] Further, the dry gel is obtained, ground, and passed through a 400-mesh sieve to obtain a precursor powder.
[0056] The present application also provides a regenerated positive electrode precursor, which is prepared by the preparation method of the regenerated positive electrode precursor described above.
[0057] The present application also provides a method for preparing a regenerated positive electrode material, comprising: sintering the regenerated positive electrode precursor mentioned above to obtain the regenerated positive electrode material.
[0058] Preferably, the powdered regenerated positive electrode precursor is sintered to obtain the regenerated positive electrode material.
[0059] According to an embodiment of the present application, the sintering is performed in an oxygen-containing atmosphere; the present application does not specifically limit the oxygen content in the oxygen-containing atmosphere, for example, the volume percentage of oxygen in the oxygen-containing atmosphere may be 0.1%-100%, for example, 0.1%, 10%, 20%, 21%, 25%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%. Further, the oxygen-containing atmosphere may be air or oxygen, and further, the partial pressure of air or oxygen may be 0.01 to 1 standard atmospheric pressure.
[0060] And / or, the sintering includes: heating the regenerated positive electrode precursor to 450-550°C (for example, 450°C, 500°C, 550°C) at a rate of 5-10°C / min (for example, 5°C / min, 8°C / min, 10°C / min), and keeping it warm for 4-6h (for example, 4h, 5h, 6h), and then heating it to 800-950°C (for example, 800°C, 850°C, 900°C, 950°C) at a rate of 5-10°C / min (for example, 5°C / min, 8°C / min, 10°C / min), and keeping it warm for 10-15h (for example, 10h, 12h, 15h); thus, under high-temperature sintering conditions, the lithium source can rearrange the structure of the waste positive electrode material and repair and regenerate the structure of the waste positive electrode material.
[0061] And / or, after the sintering is completed, the temperature is lowered to 180-220°C (e.g., 180°C, 200°C, 220°C) at a rate of 5-10°C / min (e.g., 5°C / min, 8°C / min, 10°C / min), and then cooled to room temperature to obtain the regenerated positive electrode material.
[0062] The present application also provides a regenerated positive electrode material, which is prepared by the above-mentioned method for preparing the regenerated positive electrode material. Therefore, the regenerated positive electrode material has excellent electrochemical properties.
[0063] The present application also provides a lithium-ion battery, which includes the above-mentioned regenerated positive electrode material, so that the lithium-ion battery has excellent electrochemical performance.
[0064] The present application also provides an electrical device, which includes the lithium-ion battery described above.
[0065] The electrical equipment includes mobile phones, tablets, laptops, electric toys, electric tools, battery vehicles, electric cars, ships, spacecraft, etc.
[0066] It should be noted that the term "and / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0067] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0068] Example 1
[0069] First, NCM523 (LiNi 0.5 Co 0.2 Mn 0.3 The waste battery bags of NCM523 positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were separated. The positive electrode sheets were then calcined at 550°C for 1 hour to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder. The content of metals (Li, Ni, Co, Mn) in the waste positive electrode material NCM523 was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0070] Then, 0.1 mol of waste positive electrode material powder was dispersed in 1 mol / L boric acid solution (solid-liquid ratio of 1:1 g / mL), stirred for 30 min, and then an excess of 3% LiNO3 (the ratio of the sum of the molar amount of lithium in LiNO3 and the molar amount of lithium in the waste positive electrode material NCM523 to the molar amount of non-lithium metal in the waste positive electrode material was 1.03:1) was added and stirred until dissolved to form a first mixed solution.
[0071] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1:1) dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0072] The second mixed solution was placed in a 60° C. water bath and stirred for evaporation for 4 h to obtain a gel, which was then placed in a 120° C. drying oven for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0073] The regenerated cathode precursor powder was then transferred into an air atmosphere furnace, heated to 450°C at 5°C / min and kept for 6 h, then heated to 900°C at 5°C / min and kept for 10 h, then cooled to 200°C at 5°C / min, cooled to room temperature, ground and sieved to obtain the regenerated cathode material R-NCM523([Li(Ni 0.5 Co 0.2 Mn 0.3 ) 0.9 B 0.1 O2]).
[0074] Figure 1 is a scanning electron microscope image of the waste positive electrode material NCM523 in Example 1, Figure 1 It can be seen that the surface structure of the waste positive electrode material NCM523 is rough, indicating that the surface of the waste positive electrode material NCM523 is not conducive to lithium ion embedding. Figure 2 is a scanning electron microscope image of the regenerated positive electrode material R-NCM523 in Example 1, Figure 2 It can be seen that the surface structure of the regenerated positive electrode material is smooth, indicating that the rough structure of the waste positive electrode material has been repaired.
[0075] Example 2
[0076] First, NCM622 (LiNi 0.6 Co 0.2 Mn 0.2 The waste battery bags of NCM622 positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were obtained by separation. The positive electrode sheets were then calcined at 450°C for 4 hours to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder. The content of metals (Li, Ni, Co, Mn) in the waste positive electrode material NCM622 was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0077] Then, 0.1 mol of waste positive electrode material powder was dispersed in 0.02 mol / L boric acid solution (solid-liquid ratio of 1:5 g / mL), stirred for 60 min, and then an excess of 8% CH3COOLi (the ratio of the sum of the molar amount of lithium in CH3COOLi and the molar amount of lithium in the waste positive electrode material NCM622 to the molar amount of non-lithium metal in the waste positive electrode material was 1.08:1) was added and stirred until dissolved to form a first mixed solution.
[0078] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1.3:1) is dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0079] The second mixed solution was placed in a water bath at 80° C. and stirred for evaporation for 1 h to obtain a gel, which was then placed in a drying oven at 120° C. for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0080] The regenerated cathode precursor powder was then transferred into an oxygen atmosphere furnace, heated to 550°C at 10°C / min and kept for 4 h, then heated to 850°C at 10°C / min and kept for 15 h, then cooled to 200°C at 10°C / min, and then ground and sieved to obtain the regenerated cathode material R-NCM622[Li(Ni 0.6 Co 0.2 Mn 0.2 ) 0.98 B 0.02 O2].
[0081] Example 3
[0082] First, NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 The waste battery bags of NCM811 positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were obtained by separation. The positive electrode sheets were then calcined at 500°C for 2h to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder. The content of metals (Li, Ni, Co, Mn) in the waste positive electrode material NCM811 was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0083] Then, 0.1 mol of waste positive electrode material powder was dispersed in 0.25 mol / L boric acid solution (solid-liquid ratio of 1:2 g / mL), stirred for 40 minutes, and then an excess of 5% Li2CO3 (the ratio of the sum of the molar amount of lithium in Li2CO3 and the molar amount of lithium in the waste positive electrode material NCM811 to the molar amount of non-lithium metal in the waste positive electrode material was 1.05:1) was added and stirred until dissolved to form a first mixed solution.
[0084] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1.1:1) is dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0085] The second mixed solution was placed in a water bath at 80° C. and stirred for evaporation for 1 h to obtain a gel, which was then placed in a drying oven at 120° C. for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0086] The regenerated cathode precursor powder was then transferred into an oxygen atmosphere furnace, heated to 500°C at 8°C / min and kept at this temperature for 5 h, then heated to 800°C at 8°C / min and kept at this temperature for 12 h, then cooled to 200°C at 8°C / min, and then ground and sieved to obtain the regenerated cathode material R-NCM811[Li(Ni 0.8 Co 0.1 Mn 0.1 ) 0.95 B 0.05 O2].
[0087] Example 4
[0088] First, NCA (LiNi 0.8 Co 0.15 Al 0.05 The waste battery bags of NCA positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were obtained by separation. The positive electrode sheets were then calcined at 500°C for 2h to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder. The content of metals (Li, Ni, Co, Al) in the waste positive electrode material NCA was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0089] Then, 0.1 mol of waste positive electrode material powder is dispersed in 0.25 mol / L boric acid solution (solid-liquid ratio is 1:2 g / mL), stirred for 40 min, and then an excess of 5% LiOH·H2O (the ratio of the sum of the molar amount of lithium in LiOH·H2O and the molar amount of lithium in the waste positive electrode material NCA to the molar amount of non-lithium metal in the waste positive electrode material is 1.05:1) is added and stirred until dissolved to form a first mixed solution.
[0090] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1.1:1) is dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0091] The second mixed solution was placed in a water bath at 80° C. and stirred for evaporation for 1 h to obtain a gel, which was then placed in a drying oven at 120° C. for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0092] The regenerated cathode precursor powder was then transferred into an oxygen atmosphere furnace, heated to 500°C at 8°C / min and kept at this temperature for 5 h, then heated to 800°C at 8°C / min and kept at this temperature for 12 h, then cooled to 200°C at 8°C / min, and then ground and sieved to obtain the regenerated cathode material R-NCA[Li(Ni 0.8 Co 0.15 Al 0.05 )0.95 B 0.05 O2].
[0093] Example 5
[0094] First, the waste battery bags containing LCO (LiCoO2) positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were obtained by separation. The positive electrode sheets were then calcined at 500°C for 2h to allow the powder to fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain waste positive electrode material powder. The content of metals (Li, Co) in the waste positive electrode material LCO was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0095] Then, 0.1 mol of waste positive electrode material powder is dispersed in 0.25 mol / L boric acid solution (solid-liquid ratio is 1:2 g / mL), stirred for 40 minutes, and then an excess of 5% Li2CO3 (the ratio of the sum of the molar amount of lithium in Li2CO3 and the molar amount of lithium in the waste positive electrode material LCO to the molar amount of non-lithium metal in the waste positive electrode material is 1.05:1) is added and stirred until dissolved to form a first mixed solution.
[0096] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1.1:1) is dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0097] The second mixed solution was placed in a water bath at 80° C. and stirred for evaporation for 1 h to obtain a gel, which was then placed in a drying oven at 120° C. for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0098] The regenerated cathode precursor powder was then transferred into an oxygen atmosphere furnace, heated to 500°C at 8°C / min and kept at this temperature for 5 h, then heated to 950°C at 8°C / min and kept at this temperature for 12 h, then cooled to 200°C at 8°C / min, and then ground and sieved to obtain the regenerated cathode material R-LCO[LiCo 0.95 B 0.05 O2].
[0099] Comparative Example 1
[0100] First, NCM523 (LiNi 0.5 Co 0.2 Mn 0.3The waste battery bags of NCM523 positive electrode materials were disassembled under an inert atmosphere and the positive electrode sheets were separated. The positive electrode sheets were then calcined at 550°C for 1 hour to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder. The content of metals (Li, Ni, Co, Mn) in the waste positive electrode material NCM523 was determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0101] Then, 0.1 mol of waste positive electrode material powder is dispersed in a deionized water solution (solid-liquid ratio is 1:1 g / mL), and an excess of 3% LiNO3 (the ratio of the sum of the molar amount of lithium in LiNO3 and the molar amount of lithium in the waste positive electrode material NCM523 to the molar amount of non-lithium metal in the waste positive electrode material is 1.03:1) is added and stirred until dissolved to form a first mixed solution.
[0102] Citric acid (n 柠檬酸 :n 非锂金属+锂源 =1:1) dissolved in deionized water to form a citric acid solution. The citric acid solution is added dropwise to the first mixed solution and stirred evenly to form a second mixed solution.
[0103] The second mixed solution was placed in a 60° C. water bath and stirred for evaporation for 4 h to obtain a gel, which was then placed in a 120° C. drying oven for 10 h, ground and sieved (400 mesh) to obtain a regenerated positive electrode precursor powder.
[0104] The regenerated cathode precursor powder was then transferred into an air atmosphere furnace, heated to 450°C at 5°C / min and kept for 6 h, then heated to 900°C at 5°C / min and kept for 10 h, then cooled to 200°C at 5°C / min, cooled to room temperature, ground and sieved to obtain the regenerated cathode material R-NCM523 (LiNi 0.5 Co 0.2 Mn 0.3 O2).
[0105] Figure 3 This is a scanning electron microscope image of the regenerated positive electrode material R-NCM523 in Comparative Example 1. Figure 3 It can be seen that the surface layer of the regenerated positive electrode material in Comparative Example 1 is relatively rough, indicating that the degree of repair is poor.
[0106] The regenerated positive electrode materials of Examples 1-5 and Comparative Example 1 were assembled into batteries and performance tested. Specifically, according to the mass ratio of 90:5:5 of the regenerated positive electrode materials, conductive agent (Super P) and binder (PVDF (polyvinylidene fluoride) dissolved in NMP (N-methylpyrrolidone) with a mass fraction of 5%) of Example 1 to Comparative Example 1, the corresponding mass of materials were weighed into a stirring box; the stirring box was placed in a homogenizer with a set program to mix the materials, and then evenly coated on a 16μm aluminum foil by a coating machine, and the coating thickness was controlled at 0.25mm. After drying, cutting, weighing and pressing, a positive electrode sheet with a diameter of 14mm was obtained. Metal lithium was used as the negative electrode, and a CR2032 button battery was assembled using LiPF6 / EC / EMC electrolyte and PE diaphragm.
[0107] After the button cell was placed for 10 hours, it was placed on a blue battery tester (CT2001C) for charge and discharge cycle performance test. The test conditions were set at: 25°C, 2.8-4.3V, and the button half-cell was activated by 0.1C / 0.1C cycle for 3 weeks, and then the specific capacity and cycle performance of the positive electrode material were examined by 1C / 1C cycle for 200 weeks. The specific electrochemical performance is shown in the table below.
[0108] Table 1 Performance test table of regenerated positive electrode materials of Examples 1-5 and Comparative Example 1
[0109]
[0110]
[0111] Among them, the 200 cycle performance refers to the capacity retention rate of the positive electrode material after 200 cycles of charge and discharge.
[0112] No boric acid solution was added to the preparation method of Comparative Example 1, and other conditions were the same as those of Example 1. As can be seen from Table 1, the waste positive electrode materials of Examples 1-3 and Comparative Example 1 are all NCM materials (nickel cobalt manganese oxide lithium), and the first discharge capacity, first charge and discharge efficiency, and 200 cycle performance of the regenerated positive electrode materials of Examples 1-3 are all better than those of Comparative Example 1. This shows that in the preparation method of the regenerated positive electrode material, the addition of boric acid solution can significantly improve the performance of the positive electrode material, that is, the regenerated positive electrode material prepared by the method of the present application has excellent performance. The waste positive electrode material of Example 4 is nickel cobalt aluminum oxide lithium, and the waste positive electrode material of Example 5 is lithium cobalt oxide. Examples 4-5 have the same first discharge capacity, first charge and discharge efficiency, and 200 cycle performance as Examples 1-3, indicating that when the waste positive electrode material is nickel cobalt manganese oxide lithium, nickel cobalt aluminum oxide lithium or lithium cobalt oxide, the regenerated positive electrode material prepared by the method of the present application can have excellent performance.
[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a regenerated positive electrode precursor, characterized in that: include: Mixing the waste positive electrode material with a boric acid solution, and then adding a lithium source to obtain a first mixed solution; mixing the first mixed solution with a chelating agent to obtain a second mixed solution; The regenerated positive electrode precursor is obtained by heating and drying the second mixed liquid.
2. The method for preparing a regenerated positive electrode precursor according to claim 1, characterized in that: The waste positive electrode material includes any one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium cobalt oxide; And / or, the concentration of the boric acid solution is 0.02-1 mol / L; And / or, the waste positive electrode material and the boric acid solution are mixed for 30 to 60 minutes; And / or, the solid-to-liquid ratio of the waste positive electrode material to the boric acid solution is 1:(1-5) g / mL; And / or, the waste positive electrode material is prepared by the following method: disassembling and separating waste lithium-ion batteries to obtain positive electrode sheets, calcining the positive electrode sheets at a temperature of 450 to 550° C. for 1 to 4 hours, and the waste positive electrode material falls off from the current collector to obtain the waste positive electrode material.
3. The method for preparing a regenerated positive electrode precursor according to claim 2, characterized in that: The lithium source includes a lithium salt or a hydrate of the lithium salt, and the lithium salt includes any one of LiOH, Li2CO3, LiNO3, CH3COOLi, LiCl, and Li2SO4; And / or, the ratio of the sum of the molar amount of lithium in the lithium source and the molar amount of lithium in the waste positive electrode material to the molar amount of non-lithium metal in the waste positive electrode material is (1.03-1.08):1; and / or, the molar amount of the chelating agent is 1.0 to 1.3 times the sum of the molar amount of the non-lithium metal in the waste positive electrode material and the molar amount of lithium in the lithium source; And / or, the chelating agent includes at least one of citric acid, maleic acid, malic acid, and oxalic acid.
4. The method for preparing a regenerated positive electrode precursor according to any one of claims 1 to 3, characterized in that: The preparation of the regenerated positive electrode precursor comprises: firstly heating the second mixed liquid to form a gel, and then drying the gel to obtain the regenerated positive electrode precursor; And / or, the forming of gel comprises: stirring the second mixed solution at a temperature of 60 to 80° C. for 1 to 4 hours to form a gel; And / or, the temperature of the drying process is 110-130°C; And / or, the drying process is performed for 9 to 11 hours.
5. A regenerated positive electrode precursor, characterized in that: The regenerated positive electrode precursor is prepared by the method for preparing a regenerated positive electrode precursor according to any one of claims 1 to 4.
6. A method for preparing a regenerated positive electrode material, characterized in that: include: The regenerated positive electrode precursor according to claim 5 is sintered to obtain the regenerated positive electrode material.
7. The method for preparing a regenerated positive electrode material according to claim 6, characterized in that: The sintering is carried out in an oxygen-containing atmosphere; And / or, the sintering includes: heating the regenerated positive electrode precursor to 450-550° C. at a rate of 5-10° C. / min, and keeping the temperature for 4-6 hours, and then heating the regenerated positive electrode precursor to 800-950° C. at a rate of 5-10° C. / min, and keeping the temperature for 10-15 hours; And / or, after the sintering is completed, the temperature is lowered to 180-220° C. at a rate of 5-10° C. / min, and then cooled to room temperature to obtain the regenerated positive electrode material.
8. A regenerated positive electrode material, characterized in that: The regenerated positive electrode material is prepared by the method for preparing the regenerated positive electrode material according to claim 6 or 7.
9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the regenerated positive electrode material according to claim 8.
10. An electrical device, characterized in that: The electrical equipment comprises the lithium-ion battery according to claim 9.
Citation Information
Patent Citations
Process for recycling and regenerating lithium cobalt oxide in waste lithium cobalt oxide battery
CN110010991A
Recovery and regeneration method of ternary positive electrode material of waste power lithium ion battery
CN110061319A
Method for recycling valuable metals of waste lithium ion battery and regenerating ternary positive electrode material
CN112194201A
Recycling method of nickel cobalt lithium manganate battery, regenerated nickel cobalt lithium manganate material and application
CN113113690A