Ammonium ion modified Prussian blue sodium ion battery positive electrode material and preparation method thereof
Through the ammonium ion modification method, the structural stability of the positive electrode material of Prussian blue sodium ion battery is enhanced, and the instability problem caused by crystallization water or defects in water synthesis of Prussian blue materials is solved, thereby improving the cycle stability of the battery and overall properties of the material.
Patent Information
- Application Number
- CN202410995353.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
The positive electrode material of Prussian blue sodium ion battery is unstable due to crystallization water or defects during the water system synthesis process, which reduces the cyclic stability of the battery.
The ammonium ion modification method is adopted to treat the suspension in an ultrasonic machine and heat and stir under a protective atmosphere to form hydrogen bonds between NH4+ and C≡N, which enhances the stability of the crystal structure and deionizes it. Cleaning and vacuum drying of water and anhydrous ethanol to obtain modified Prussian blue compounds.
Improve the cyclic stability and overall crystallinity of Prussian blue sodium electropositive electrode materials, ensure the structural stability of the material during charging and discharging, and make the particle size of the material smaller and more uniform, enhancing the contact performance with the electrolyte .
Smart Images

Figure CN118954538A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion battery positive electrode materials, and specifically refers to an ammonium ion-modified Prussian blue sodium ion battery positive electrode material and a preparation method thereof. Background Art
[0002] Due to the rapid development of lithium-ion battery technology, the application of lithium-ion batteries has grown rapidly. However, the global distribution of lithium resources is extremely uneven and the reserves are small, which leads to the high price of lithium-ion batteries. Since sodium reserves are abundant and widely distributed around the world, sodium-ion batteries that achieve energy storage through sodium ion conduction have attracted widespread attention and have important application prospects in the fields of large-scale energy storage, low-speed electric vehicles, and two-wheel electric vehicles. Prussian blue compounds are important positive electrode materials for sodium-ion batteries because of their spacious sodium ion channels. However, because their synthesis process is carried out in an aqueous system, their crystal structure usually contains a certain amount of crystal water or defects, which leads to instability of the crystal structure when sodium ions are deintercalated, thereby reducing the cycle stability of such batteries. Therefore, obtaining structurally stable Prussian blue compounds is an important guarantee for improving their sodium-ion batteries. Summary of the invention
[0003] The purpose of the present invention is to address the shortcomings of the traditional liquid phase coprecipitation method for synthesizing Prussian blue compounds, and to propose a structure-stable Prussian blue compound positive electrode material modified with ammonium ions and a preparation method of the material. + The formation of new hydrogen bonds between the N atoms in C≡N enhances the stability of the crystal structure, thereby improving the cycle stability of this type of battery.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a Prussian blue type sodium ion battery positive electrode material modified by ammonium ions and a preparation method thereof, the preparation method comprising the following steps:
[0005] (1) Stir the ammonium salt under a protective atmosphere to obtain NH4 + Solution;
[0006] (2) Add the Prussian blue compound prepared by the traditional liquid phase coprecipitation method to NH4 + A suspension is formed in the solution.
[0007] (3) Ultrasonicate the suspension obtained in step (2) in an ultrasonic machine.
[0008] (4) heating and stirring the suspension obtained in step (3), cooling and aging the suspension.
[0009] (5) The precipitate obtained in step (4) is washed with deionized water and anhydrous ethanol and dried in vacuum to obtain a modified Prussian blue compound. The hydrogen bonds formed in the crystal structure of the material play a stabilizing role in the structure.
[0010] Preferably, in step (1), the ammonium salt is one or more of ammonium fluoride, ammonium dihydrogen phosphate, ammonium ferrous sulfate, ammonium persulfate and the like; the NH4 + The concentration is 0.01~0.5mol / L.
[0011] Preferably, in step (1), the solvent is deionized water, and a surfactant may be added, such as hexadecyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, and octadecyldimethylhydroxyethylammonium nitrate.
[0012] Preferably, in step (1), an organic sodium salt or an inorganic sodium salt additive may be added to the solution, such as one or more of trisodium citrate, sodium ascorbate, sodium chloride, sodium sulfate, sodium carbonate, sodium acetate, or sodium nitrate.
[0013] Preferably, in step (2), the unmodified Prussian blue compound material has the general structural formula: Na x M (1-m) Fe m [N(CN)4] n , where: x is 0.01~3.0, m is 0~1, n is 0~1, and M and N are any one or more of Fe, Co, Ni, Mn, Cu, and Zn.
[0014] Preferably, in the step (4), the ventilation heating and rotation time is 1 to 48 hours; and the natural aging time is 1 to 48 hours.
[0015] Preferably, in the step (5), the vacuum drying temperature is 70 to 150° C., and the drying time is 8 to 48 hours.
[0016] Furthermore, the present invention also uses the modified Prussian blue compound as a positive electrode material for a sodium ion battery to prepare a sodium ion battery, thereby improving the cycle performance of the battery.
[0017] The beneficial effects achieved by the present invention using the above structure are as follows:
[0018] (1) Modified Prussian blue compound NH4 + New hydrogen bonds are formed between the N atoms in C≡N, and the new structure makes the material more stable; it ensures that the modified Prussian blue sodium-based positive electrode material has a more stable charge and discharge structure, thereby improving the cycle stability of the sodium-ion battery.
[0019] (2) The modified Prussian blue sodium cathode material transforms from a monoclinic phase to a cubic phase with a better symmetrical structure, thereby improving the overall crystallinity of the material.
[0020] (3) Under the weak acidic effect of ammonium salt, the particle size of the modified Prussian blue compound becomes smaller and more uniform, which is beneficial for the contact between the material and the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Comparison curve of the cycle performance of the half-cell assembled with the material N0 before modification and the material N1 obtained in Example 1 at 50°C;
[0022] Figure 2 XRD patterns of material N0, Example 1 and Example 2 before modification;
[0023] Figure 3 Scanning electron microscope image (SEM) of material N0 before modification according to the present invention;
[0024] Figure 4 Figure 3 Energy dispersive X-ray spectrometry (EDS) of selected areas;
[0025] Figure 5 Scanning electron microscope image (SEM) of material N1 obtained in Example 1 of the present invention;
[0026] Figure 6 Figure 5 Energy dispersive X-ray spectroscopy (EDS) of selected areas.
[0027] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0030] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.
[0031] In the present invention, the ammonium salt is one or more of ammonium fluoride, ammonium dihydrogen phosphate, ammonium ferrous sulfate, ammonium persulfate and the like. The surfactant is one or more of hexadecyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, octadecyldimethylhydroxyethylammonium nitrate and the like. The sodium additive is one or more of sodium chloride, sodium sulfate, sodium carbonate, sodium acetate, trisodium citrate, sodium ascorbate or sodium nitrate and the like. The general structural formula of the unmodified Prussian blue sodium positive electrode material is: Na x M (1-m) Fe m [N(CN)4] n , wherein: x is 0.01-2.0, m is 0-1, n is 0-1, and M and N are any one or more of Fe, Mn, Mg, Cs, Ti, Ni, Cu, Zn, and Co. The unmodified Prussian blue compound used in the embodiment of the present invention is a manganese-doped iron-based Prussian blue compound.
[0032] Example 1
[0033] A kind of ammonium ion modified Prussian blue type sodium ion battery positive electrode material and preparation method thereof
[0034] (1) 1.2 g of unmodified manganese-doped iron-based Prussian blue material (labeled as: N0) was dispersed in 50 ml of deionized water to form a suspension A;
[0035] (2) dissolving 0.05 M NH4F, 0.3 g dodecyldimethylbenzyl ammonium chloride and 2 g sodium carbonate in 150 ml of deionized water to form aqueous solution B, and adding the aqueous solution B to suspension A to obtain suspension C;
[0036] (3) The suspension C was heated at 90°C and stirred at 300 rpm for 12 h under the condition of blowing N2, and then aged for 5 h; then, it was centrifuged and washed with a mixed solution of deionized water and anhydrous ethanol for more than 3 times to obtain a light blue precipitate;
[0037] (4) The precipitate was placed in a vacuum oven and dried at 110° C. for 24 h to obtain a modified manganese-doped iron-based Prussian blue positive electrode material labeled as N1.
[0038] Example 2
[0039] A kind of ammonium ion modified Prussian blue type sodium ion battery positive electrode material and preparation method thereof
[0040] (1) dispersing 1.2 g of unmodified manganese-doped iron-based Prussian blue material N0 in 50 ml of deionized water to form a suspension A;
[0041] (2) dissolving 0.05 M (NH4)2HPO4, 0.3 g polyvinyl pyrrolidone and 2 g NaCl in 150 ml of deionized water to form aqueous solution B, and adding the aqueous solution B to suspension A to obtain suspension C;
[0042] (3) The suspension C was heated at 60°C and stirred at 300 rpm for 12 h under the condition of blowing N2, and then aged for 5 h; then, it was centrifuged and washed with deionized water and anhydrous ethanol for more than 3 times to obtain a light blue precipitate;
[0043] (4) The precipitate was placed in a vacuum oven and dried at 140° C. for 24 h to obtain a modified manganese-doped iron-based Prussian blue positive electrode material labeled as N2.
[0044] Example 3
[0045] A kind of ammonium ion modified Prussian blue type sodium ion battery positive electrode material and preparation method thereof
[0046] (1) dispersing 1.2 g of unmodified manganese-doped iron-based Prussian blue material N0 in 50 ml of deionized water to form a suspension A;
[0047] (2) dissolving 0.05 M (NH4)2FeSO4, 0.3 g polyvinyl pyrrolidone and 2 g NaCl in 150 ml of deionized water to form aqueous solution B, and adding the aqueous solution B to suspension A to obtain suspension C;
[0048] (3) The suspension C was heated at 60°C and stirred at 300 rpm for 5 h under the condition of blowing N2, and then aged for 5 h; then, it was centrifuged and washed with deionized water and anhydrous ethanol for more than 3 times to obtain a light blue precipitate;
[0049] (4) The precipitate was placed in a vacuum oven and dried at 140° C. for 24 h to obtain a modified manganese-doped iron-based Prussian blue positive electrode material labeled as N3.
[0050] Experimental Example 1
[0051] The material prepared by the process of the embodiment was used as the active material to prepare the electrode sheet for the assembly test of the sodium ion battery. The assembled half-cell was used in the constant current charge and discharge mode to carry out the corresponding electrochemical performance test.
[0052] The electrochemical performance test results of each material are shown in Table 1.
[0053] Table 1 Electrochemical performance of samples in various embodiments
[0054]
[0055] By comparison, it can be seen that the final product of Example 2 has the best electrochemical performance, and the cycle stability of the NH4+ ion-modified Prussian blue sodium ion positive electrode material during the charge and discharge process is greatly improved, indicating that the crystal structure of the material does not deform during the sodium ion insertion and extraction process.
[0056] Figure 1 The comparison curve of the 10,000-cycle performance of the half-cell assembled with the material N0 before modification and the material N1 obtained in Example 1 at 50°C shows that the capacity decay of the material N1 in Example 1 after 10,000 cycles is very small, while the capacity decay of the material N0 before modification is obvious, with a decay rate of more than 40%. Figure 2 is the XRD picture of material N0, Example 1 and Example 2 before modification; Figure 2 It can be seen that the diffraction double peak of the modified Prussian blue compound at 24.5° becomes a single peak, indicating that the iron-based Prussian white compound containing crystal water and sodium-rich monoclinic phase structure (space group is R-3) is transformed into a modified cubic center (space group is I-3) after weak acidification treatment with ammonium salt. The cubic structure has greater symmetry and the material structure is more stable. Figure 3 This is a scanning electron microscope (SEM) image of material N0 before modification according to the present invention; Figure 4 for Figure 3 Energy dispersive X-ray spectrometry (EDS) of selected areas; Figure 5 This is a scanning electron microscope (SEM) image of the material N1 obtained in Example 1 of the present invention; Figure 6 for Figure 5 Energy dispersive X-ray spectroscopy (EDS) of selected areas. Figure 3 and Figure 5 It can be clearly seen that the particle size of the Prussian blue compound modified by ammonium ions becomes smaller and more uniform; Figure 4 and Figure 6 It can be seen that the nitrogen content increases and the oxygen content becomes lower; the increase in nitrogen content is due to the insertion of NH4+, NH4 + New hydrogen bonds are formed between the N atoms in the C≡N of the Prussian blue compound. The new structure makes the crystal structure of the material more stable; the oxygen content becomes lower because NH4 + The insertion improves the overall crystallinity of the material, and the content of crystalline water is further reduced, resulting in a decrease in the oxygen content in the material.
[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0058] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.
Claims
1. A method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material, characterized in that: The preparation method comprises the following steps: (1) Add ammonium salt, surfactant and sodium additive into deionized water and stir for a suitable time under protective atmosphere to obtain ammonium ions (NH4 + ) solution; (2) Add the Prussian blue compound prepared by coprecipitation into NH4 + A suspension is formed in the solution; (3) ultrasonically cleaning the suspension obtained in step (2) in an ultrasonic machine; (4) heating and rotating the suspension obtained in step (3) while introducing nitrogen, then cooling naturally and aging; (5) The precipitate obtained in step (4) is washed with deionized water and anhydrous ethanol and vacuum-dried to obtain a modified Prussian blue compound material. The modified Prussian blue material forms new hydrogen bonds between the internal NH4+ and the N atoms in C≡N to improve the stability of the crystal structure.
2. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 1, characterized in that: In the step (1), the ammonium salt is one or more of ammonium fluoride, ammonium dihydrogen phosphate, ammonium ferrous sulfate, ammonium persulfate, etc.; the NH4 + The concentration is 0.01~0.5mol / L.
3. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 2, characterized in that: In the step (1), the surfactant is selected from one of the quaternary ammonium salt surfactants cetyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, and octadecyldimethylhydroxyethylammonium nitrate; and the mass ratio of the surfactant to the unmodified Prussian blue sodium cathode material is 0 to 0.5:
1.
4. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 3, characterized in that: In the step (1), the sodium additive is one or more of sodium chloride, sodium sulfate, sodium carbonate, sodium acetate, trisodium citrate, sodium ascorbate or sodium nitrate; and the mass ratio of the sodium additive to the unmodified Prussian blue sodium cathode material is 1 to 3:
1.
5. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 4, characterized in that: In the step (1), the protective gas includes nitrogen, argon or a mixture of the two; and the stirring time is 10 to 50 minutes.
6. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 5, characterized in that: In the step (2), the unmodified Prussian blue compound material has the general structural formula: Na x M (1-m) Fe m [N(CN)4] n , where: x is 0.01~2.0, m is 0~1, n is 0~1, and M and N are any one or more of Fe, Mn, Ni, Cu, Zn, and Co.
7. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 6, characterized in that: In the step (3), the ultrasonic time is 5 to 100 minutes.
8. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 7, characterized in that: In the step (4), the nitrogen flow rate is 5 to 100 ml / min; the heating temperature is 30 to 150° C. and the rotation speed is 100 to 2000 rpm; the reaction time is 3 to 48 hours; and the natural aging time is 3 to 48 hours.
9. The method for preparing an ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 8, characterized in that: In the step (5), the vacuum drying temperature is 90-180° C., and the drying time is 10-30 hours.
10. The ammonium ion-modified Prussian blue-based sodium ion battery cathode material according to claim 9, characterized in that: The modified Prussian blue sodium cathode material is prepared by the method according to any one of claims 1 to 9.