Impermeable material as well as preparation method and application thereof

By stirring red mud and desulfurization ash with additives such as calcium hydroxide and ball milling to form CaAl-type LDH, the problem of time-consuming and insufficient resource utilization of red mud and desulfurization ash is solved, and efficient and low-cost anti-seepage materials are prepared , used in landfill anti-seepage system, realizes the coordinated resource utilization of red mud and desulfurization ash.

CN118954564APending Publication Date: 2024-11-15FUJIAN LONGKING DSDN ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201789.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The treatment methods of red mud and desulfurization ash are time-consuming, large space-consuming, potential pollution risks, and cannot be effectively used in resource utilization, resulting in environmental and economic problems.

Method used

By stirring red mud and desulfurization ash with additives such as calcium hydroxide and other additives, and performing a mechanical chemical reaction of ball milling to form layered calcium-aluminum bimetallic hydroxide (CaAl type LDH), a high anti-seepage coefficient and compressive strength were prepared. Anti-seepage materials to realize the coordinated resource utilization of red mud and desulfurization ash.

Benefits of technology

It shortens the disposal time of red mud, saves floor area, reduces permeability, and improves crack resistance and adsorption performance. It replaces natural clay as a landfill anti-seepage material, and reduces preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of industrial waste treatment, and provides an impermeable material as well as a preparation method and application thereof. The preparation method of the impermeable material comprises the following steps: (1) stirring raw materials including red mud, desulfurized fly ash and optional additives to obtain a mixture; and (2) performing ball-milling mechanical chemical reaction on the mixture to form a layered calcium-aluminum double-metal hydroxide, thereby obtaining the impermeable material, wherein the additive comprises calcium hydroxide, and the mass content of water in the red mud is 40%-60%. The anti-seepage material uses the red mud and the desulfurized fly ash as raw materials, and cooperative treatment of the red mud and the desulfurized fly ash is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of industrial waste treatment, and specifically relates to an anti-seepage material and a preparation method and application thereof. Background Art

[0002] Red mud is an industrial solid waste generated during the alumina smelting process. According to statistics, my country's annual red mud production is about 100 million tons, of which only about 10 million tons can be effectively utilized, and the rest of the red mud is disposed of by landfill. At present, the main method of treating red mud is to pump the red mud slurry into a red mud dump or red mud dam, recover the supernatant after natural sedimentation, reuse it in the alumina smelting process, and let the remaining red mud dry naturally. After the red mud dump or red mud dam is full, it will be sealed for treatment. However, these treatment methods are time-consuming, occupy a lot of space, waste land resources, and the accumulated red mud may seep and pollute groundwater; and the fine particles in the red mud after air drying are easily blown away by the wind, polluting the air. The red mud dam also has a potential risk of dam collapse and pollute the surrounding land.

[0003] Desulfurization ash is a general industrial solid waste generated by dry or semi-dry flue gas desulfurization. With the continuous promotion of dry and semi-dry desulfurization processes, the annual output of desulfurization ash has increased year by year. Desulfurization ash contains multiple components such as calcium sulfite, calcium hydroxide, and calcium carbonate. It is currently mainly used in traditional building materials and roadbed materials such as aerated blocks, autoclaved bricks, mortar, and asphalt concrete. It is greatly affected by seasonal and regional conditions and cannot be fully utilized as a resource. It is necessary to explore new comprehensive application directions.

[0004] If the coordinated resource utilization of red mud and desulfurization ash can be achieved, it will have very important environmental and economic significance. Summary of the invention

[0005] In view of the above-mentioned problems, the purpose of this application is to provide an anti-seepage material and its preparation method and application. The preparation method of this application realizes the coordinated treatment and resource utilization of red mud and desulfurization ash, and the prepared anti-seepage material has a high anti-seepage coefficient and compressive strength.

[0006] To achieve the above-mentioned object, the first aspect of the present application provides a method for preparing an anti-seepage material, comprising: (1) mixing raw materials including red mud, desulfurization ash and optional additives to obtain a mixture; (2) subjecting the mixture to a ball milling mechanochemical reaction to form a layered calcium aluminum double hydroxide (CaAl-type LDH) to obtain the anti-seepage material; wherein: The additive comprises calcium hydroxide, and the mass content of water in the red mud is 40% to 60%.

[0007] The preparation method of the present application realizes the coordinated management and resource utilization of red mud and desulfurization ash. By controlling the water content of red mud, red mud and desulfurization ash are mechanochemically formed into an anti-seepage material containing CaAl-type LDH. Compared with directly stacking and air-drying red mud, the method of the present application can shorten the disposal time of red mud and save the area occupied by red mud; the prepared anti-seepage material has a lower permeability coefficient and has both higher adsorption and crack resistance. Its preparation cost is low and it can replace natural clay as a landfill anti-seepage material.

[0008] In some embodiments of the present application, the preparation method further comprises: subjecting the red mud slurry to sedimentation and dehydration treatment to obtain the red mud. The red mud used in the present application can be directly obtained by subjecting the red mud slurry to sedimentation and dehydration treatment to a certain degree.

[0009] In some embodiments of the present application, the mass content of water in the red mud (i.e., water content) is 44% to 52%. Controlling the water content within this range can, on the one hand, inhibit the agglomeration of raw material sludge and the difficulty in mixing components evenly due to too low a water content, and reduce the possibility of difficulty in agglomeration of desulfurized ash and difficulty in compaction in subsequent landfill construction; on the other hand, it can minimize the low plasticity of subsequent products and increased construction difficulty caused by too high a water content.

[0010] In some embodiments of the present application, on a dry basis, the mass content of aluminum oxide in the red mud is 15% to 30%, and the mass content of silicon dioxide is 20% to 50%.

[0011] In some embodiments of the present application, the mass content of calcium hydroxide in the desulfurization ash is 10%~30%, the mass content of calcium carbonate is 10%~30%, and the mass content of calcium sulfite is 25%~60%.

[0012] In some embodiments of the present application, the mass ratio of the desulfurized ash to the red mud on a dry basis is (2-3): 1. Thus, on the one hand, the desulfurized ash and the red mud can be promoted to form LDH, and on the other hand, some unreacted raw materials can be retained in the anti-seepage material, which can improve the application effect of subsequent landfill.

[0013] In some embodiments of the present application, the additive is carbide slag, and the mass content of calcium hydroxide in the carbide slag is ≥80%.

[0014] In some embodiments of the present application, the amount of the additive is 0-10% based on the total mass of the desulfurization ash and the red mud on a dry basis.

[0015] In some embodiments of the present application, in the mixture, the mass ratio of calcium hydroxide to aluminum oxide is (3-4):1, and the mass ratio of calcium carbonate to aluminum oxide is (0.5-5):1.

[0016] In some embodiments of the present application, based on the total mass of the red mud and the desulfurization ash, the mass content of water in the mixture is 18% to 40%, preferably 21% to 30%.

[0017] In some embodiments of the present application, in the ball milling mechanochemical reaction, the ball mill speed rate is 76% to 88%, and the ball milling time is 30 min to 100 min.

[0018] Furthermore, the ball milling time is 40 min to 80 min. This can further improve the anti-seepage performance of the anti-seepage material.

[0019] The second aspect of the present application provides an anti-seepage material prepared by the preparation method described in the first aspect of the present application.

[0020] The anti-seepage material prepared in the present application includes CaAl type LDH. Under the action of mechanical grinding, the aluminum oxide and calcium hydroxide in the red mud and desulfurization ash are changed from a stable crystalline state to an unstable state with weaker crystallinity. This process is accompanied by the breaking of a large number of chemical bonds and the generation of defects on the microscopic surface of the particles, the generation and release of various active functional groups and free radicals, and the removal of crystal water, which continuously generates a mineral surface with high chemical reactivity, promotes the reaction generation, and the calcium carbonate and calcium sulfite in the desulfurization ash can provide CO3 2- and SO3 2- Anions, CO3 during ball milling 2- and SO3 2- It can enter the LDH structure in the form of interlayer anions to generate stable CaAl-type LDH. The anti-seepage material prepared in this application has a high anti-seepage coefficient and compressive strength. In addition, after the anti-seepage material is applied to the landfill and compacted during construction, the unreacted desulfurization ash and red mud can gradually generate calcium silicate and slightly expansive calcium sulfonate, which reduces the permeability coefficient of the anti-seepage layer.

[0021] The third aspect of the present application provides the use of the anti-seepage material in a landfill anti-seepage system.

[0022] The anti-seepage material of the present application can be used in the anti-seepage system of the landfill. After the anti-seepage material is compacted during construction, the CaAl type LDH therein has strong water absorption and adsorption performance, and the LDH has a lamellar structure, and the lateral tensile performance is stronger, so that the soil is not easy to crack. In addition, the unreacted desulfurization ash has a large specific surface area due to its small fineness, which is also conducive to improving the water absorption effect of the material, and the hemihydrate calcium sulfite and calcium hydroxide in the desulfurization ash will also react with the aluminum oxide of the red mud to generate calcium sulfonite, which provides a certain strength for the anti-seepage system. And because of the presence of more calcium sulfite, the reaction process of this hydration reaction is slow and long-term, which can gradually reduce the free water in the system, reduce the penetration risk of the permeate, and improve the anti-seepage performance and the strength in the later application process.

[0023] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. DETAILED DESCRIPTION

[0024] The following describes the implementation of the present application in detail. The implementation described below is exemplary and is only used to explain the present application, and cannot be understood as limiting the present application.

[0025] The "range" disclosed in the present application is defined in the form of a lower limit and / or an upper limit, and a given range is defined by selecting a lower limit and / or an upper limit. The range defined in this way can be inclusive or exclusive of end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form an unclearly recorded range, and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, each separately disclosed point or single value itself can be combined with any other point or single value as a lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0026] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0027] In a first aspect, the present application provides a method for preparing an anti-seepage material, comprising the following steps: (1) mixing raw materials including red mud, desulfurization ash and optional additives to obtain a mixture; (2) subjecting the mixed material to a ball milling mechanochemical reaction to form a layered calcium aluminum double hydroxide (CaAl-type LDH) to obtain the anti-seepage material.

[0028] Red mud, also known as red mud, is an industrial solid waste discharged after the extraction of alumina from bauxite. Generally, the main chemical components of red mud include silicon dioxide, aluminum oxide, iron oxide, calcium oxide, etc.

[0029] According to the method of the present application, the red mud may be red mud produced by the Bayer process. According to some embodiments, on a dry basis, the mass content of aluminum oxide (Al2O3) in the red mud is 15% to 30%, and the mass content of silicon dioxide (SiO2) is 20% to 50%. It is understandable that "on a dry basis" refers to the total amount of red mud (i.e., red mud dry sample) excluding water. For example, "on a dry basis, the mass content of Al2O3 in red mud is 15%" means that the mass content of Al2O3 is 15% based on the weight of the red mud dry sample. As some examples, on a dry basis, the mass content of calcium oxide (CaO) in the red mud is 10% to 22%, and the mass content of iron oxide (Fe2O3) is 18% to 32%. The chemical composition of the red mud mentioned in the present application is calculated after analyzing the elements using X-ray fluorescence spectrometry (XRF).

[0030] According to the method of the present application, the water content of the red mud used to prepare the anti-seepage material is 40% to 60%, such as 40%, 42%, 44%, 45%, 48%, 50%, 52%, 55%, 56%, 60%, etc. The inventors of the present application found in their research that if the water content is too low, it is difficult to mix the raw materials evenly during stirring, and insufficient water during ball milling will affect the dissolution of anions and embedding between the formed LDH slabs, making the generated LDH less stable; if the water content is too high, the product generated after ball milling is in a slurry state and is difficult to use directly, and requires additional dehydration.

[0031] Preferably, the water content of the red mud is 44% to 52%. In this case, on the one hand, the raw material sludge can be inhibited from agglomerating, stirring can be uniform, and the desulfurized ash can be agglomerated into agglomerates; on the other hand, the plasticity of subsequent products can be improved and the construction difficulty can be reduced.

[0032] According to the method of the present application, the red mud can be provided by red mud slurry. According to some embodiments, the preparation method further comprises the step of preparing the red mud: subjecting the red mud slurry to sedimentation and dehydration treatment to obtain the red mud.

[0033] Generally, the water content of the red mud slurry (i.e., wastewater containing red mud) produced during the red mud smelting process is not less than 97%. As some examples, the red mud slurry can be transported to a sedimentation tank for sedimentation treatment to be initially dehydrated to obtain a sediment (the water content is generally 75% to 90%), and then a dehydrator is used to dehydrate the sediment to obtain red mud with the required water content. The dehydrator can be selected from one or more of a plate and frame filter press, a belt dehydrator, a centrifugal dehydrator, and a stacked dehydrator.

[0034] In some embodiments, the proportion of particles with a particle size of less than 25 μm in the red mud (on a dry basis) is greater than 70%. In this way, the reactivity of the red mud can be increased.

[0035] According to the method of the present application, the desulfurization ash may be dry desulfurization ash. Dry desulfurization ash refers to a calcium-based powdered mixture rich in calcium sulfite, calcium sulfate, calcium carbonate, calcium hydroxide, etc. produced by dry / semi-dry desulfurization processes such as circulating fluidized bed (CFB), new integrated desulfurization (NID) or rotary spray drying absorption (SDA). In addition, the dry desulfurization ash produced by power plants and coal-fired boilers also contains silicon dioxide, aluminum oxide and iron oxide.

[0036] According to some embodiments, the mass content of calcium hydroxide (Ca(OH)2) in the desulfurized ash is 10%~30%, the mass content of calcium carbonate (CaCO3) is 10%~30%, and the mass content of calcium sulfite (CaSO3) is 25%~60%.

[0037] In some embodiments, the mass proportion of particles with a particle size of less than 25 μm in the desulfurized ash used is more than 75%. In this way, the reactivity of the particles with red mud can be improved, the time and energy consumption required for grinding materials in the ball milling reaction can be saved, and the ball milling process can be mainly used for the reaction between materials.

[0038] According to the method of the present application, the amount of the red mud and the desulfurized ash can be selected in combination with their respective compositions and the calcium hydroxide and aluminum oxide required for synthesizing LDH. According to some embodiments, the mass ratio of the desulfurized ash to the red mud on a dry basis is (2-3):1, for example, 2:1, 2.2:1, 2.5:1, 2.7:1, 3:1, etc.

[0039] In some embodiments, based on the total mass of the red mud and the desulfurized ash, the mass content of water in the mixture is 18% to 40%, preferably 21% to 30%. It can be understood that "based on the total mass of the red mud and the desulfurized ash" means that when the mixture also contains additives, the mass of the additives is not taken into account when calculating the moisture content of the mixture.

[0040] In some embodiments, in the mixture, the mass ratio of calcium hydroxide to aluminum oxide is (3-4): 1, and the mass ratio of calcium carbonate to aluminum oxide is (0.5-5): 1, preferably (1.5-3.5): 1. It should be understood that when calculating the mass ratio of chemical components in the mixture, the mass of aluminum oxide is provided by red mud, and the mass of calcium carbonate is provided by desulfurization ash; in addition, although calcium hydroxide is mainly provided by desulfurization ash and additives, the calcium oxide in the red mud needs to be taken into account when calculating the mass of calcium hydroxide. Specifically, when the mass of calcium oxide in the red mud is m, the corresponding calcium hydroxide provided by the red mud is 1.32m (1.32 is the molar mass ratio of calcium hydroxide to calcium oxide).

[0041] According to the method of the present application, the additive is a raw material containing calcium hydroxide, for example, calcium hydroxide, or waste residue containing calcium hydroxide. The waste residue containing calcium hydroxide may include carbide slag, and the mass content of calcium hydroxide in the carbide slag is usually not less than 75%.

[0042] In some embodiments, the additive is carbide slag, and the mass content of calcium hydroxide in the carbide slag is ≥80%, for example, 80%, 81%, 82%, 85%, 90%, etc.

[0043] According to the method of the present application, the additive may or may not be used in step (1). The additive is intended to make up for the calcium hydroxide required for synthesizing LDH to obtain a suitable calcium-aluminum ratio.

[0044] According to some embodiments, based on the total mass of the desulfurization ash and the red mud on a dry basis, the amount of the additive is 0-10%, for example, 1%, 2%, 3%, 4%, 7%, 8%, etc.

[0045] In step (1), the present application does not particularly limit the stirring method, as long as the components can be mixed evenly, the stirring can be carried out in various mixers, such as drum mixers, twin-shaft mixers, vertical mixers, etc. Preferably, a twin-shaft mixer is used for stirring to further improve the dispersion uniformity of the components. Generally, the stirring time can be set to 10 min to 30 min.

[0046] According to the method of the present application, in step (2), the obtained mixture is ball-milled to perform a mechanochemical reaction to generate a layered calcium aluminum double hydroxide (CaAl-type LDH). It can be understood that the mechanochemical method uses mechanical energy to stimulate the interaction between material molecules to achieve chemical reaction drive.

[0047] Layered double hydroxide (LDH) is an inorganic functional material with a layered structure, which consists of a positively charged main layer and anions and water molecules between the layers. The chemical composition of LDH can be expressed as [M1-x 2+ Mx 3+ (OH)2] x+ [A n- ] x / n mH2O, where M 2+ and M 3+ represents divalent and trivalent metal cations (M in this application 2+ 、M 3+ Represents Ca 2+ 、Al 3 + ), and OH - Together they form the cationic layer or main layer of LDH, with anions between the layers, which have strong adsorption capacity.

[0048] The traditional method for preparing LDH mineral materials is a simultaneous precipitation process, a hydrothermal method and a urea reduction process. Since Ca and Al in desulfurization ash and red mud exist in the form of oxides and hydroxides rather than ions, it is difficult to synthesize LDH using the above conventional methods. In step (2) of the present application, the mechanochemical method can continuously generate a fresh mineral surface with high chemical reactivity on a macro scale, promote the solid phase reaction to directly form LDH, and this method is a one-step method for generating LDH, without the need for additional water addition and subsequent dehydration operations, and the preparation process is simple.

[0049] In some embodiments, in the ball milling mechanochemical reaction, the ball mill speed rate is 76% to 88%, and the ball milling time is 30 min to 100 min.

[0050] Preferably, the ball milling time is 40 min to 80 min. This can improve the degree of reaction while avoiding the situation where the particle size of the anti-seepage material is too small due to the ball milling time being too long, so that the reaction speed is too fast during the application process.

[0051] According to the method of the present application, the obtained product can be characterized by XRD test. The results show that relatively obvious diffraction peaks appear near 2θ angles of 10.26°, 20.60°, and 31.11°, respectively. These three diffraction peaks correspond to (001), (002), and (110) lattice planes, respectively, indicating that LDH has been successfully synthesized. Under the action of mechanical grinding, Al2O3 and Ca(OH)2 in red mud and desulfurization ash change from a stable crystalline state to an unstable state with weaker crystallinity. This process is accompanied by the breaking of a large number of chemical bonds and the generation of defects on the microscopic surface of the particles, the generation and release of various active functional groups and free radicals, and the removal of crystal water, which continuously generates a mineral surface with high chemical reactivity and promotes the reaction generation. However, mechanical grinding of Al2O3 and Ca(OH)2 alone is more likely to form hydrogrossular minerals rather than LDH, which do not have a stable lamellar structure and anion exchange capacity, and a third phase calcium salt must be introduced to provide negative ions between slabs; calcium carbonate and calcium sulfite in desulfurization ash can effectively provide anions CO3 2- and SO3 2- , CO3 2- 、SO3 2- It can enter the LDH structure in the form of interlayer anions, so that it can react to generate a stable CaAl-type LDH after mechanical grinding, thereby obtaining the barrier material containing the CaAl-type LDH.

[0052] In a second aspect, the present application provides an anti-seepage material prepared by the preparation method of the first aspect of the present application.

[0053] Generally, the impermeable material may include CaAl-type LDH, unreacted red mud and unreacted desulfurization ash. After the impermeable material is compacted as the impermeable layer of the landfill, other reactions will occur, such as hydration reaction: the hemihydrate calcium sulfite (CaSO3·2H2O) and calcium hydroxide provided by the desulfurization ash will react with the alumina provided by the red mud to form calcium sulfonite, providing a certain strength. Because of the presence of more calcium sulfite, the hydration reaction is slow and long-term, which is conducive to the construction and application of the impermeable material, and can gradually reduce the free water in the system. This feature is conducive to improving the later strength of the impermeable layer (if the reaction speed is fast, it will harden and agglomerate in advance, which is not conducive to the formation of a dense impermeable layer during the compaction process during the landfill construction, and will lead to a reduction in the later strength improvement of the entire landfill impermeable layer). In addition, the desulfurization ash has a small fineness, a large specific surface area, and a strong water absorption performance.

[0054] In a third aspect, the present application provides the application of the anti-seepage material described in the second aspect of the present application in a landfill anti-seepage system.

[0055] With the construction of urbanization, the amount of domestic waste treatment is also increasing, and the number of domestic waste landfills has increased significantly year by year. In order to prevent the leachate of landfill waste from penetrating into the soil and groundwater, it is necessary to lay an impermeable layer on the bottom of the landfill. The construction of traditional landfills requires the laying of impermeable layers on the lower and upper layers of the landfill body. The lower impermeable layer prevents the leachate in the landfill body from penetrating into the natural soil and polluting the environment. The upper impermeable layer prevents rainwater from infiltrating into the landfill body after the landfill is filled and sealed. Usually, the impermeable layer adopts a combination of one or more layers of HDPE geomembrane and natural clay liner. The permeability coefficient of natural clay is required to be less than 1×10 -7 cm / s. The laying of the landfill anti-seepage layer requires a large amount of natural clay. As the number of landfills increases, the demand for natural clay is also increasing, but the price of natural clay is not low, and excessive exploitation of natural clay will also cause damage to local vegetation and geological landforms. The anti-seepage material of this application can replace natural clay as an anti-seepage layer material.

[0056] In some embodiments, the applying includes: compacting the anti-seepage material to form an anti-seepage layer.

[0057] According to the application of this application, the LDH in the anti-seepage material provides strong water absorption and adsorption performance (the anions between the LDH slabs can be replaced with the anions in the organic pollutants, and the organic anions are fixed in the slab structure, and no longer seep down, which plays an effective adsorption role), and the LDH interlayer can adsorb free water, so that the whole system is not easy to shrink. Since the LDH is a lamellar structure, the lateral tensile resistance is stronger, making the system less prone to cracking macroscopically. In addition, the silicon, aluminum, and iron components in the red mud will gradually react with the calcium-based compounds in the desulfurization ash, and after the above-mentioned ball milling, the activity of the reaction is higher, and calcium silicate and calcium sulfonate with a certain strength are generated. Moreover, under the retarding effect of calcium sulfite, the generation of calcium silicate and calcium sulfonate is a long and slow process. With the generation of calcium silicate and calcium sulfonate, the volume of calcium sulfonate in the soil increases and there will be a certain degree of micro-expansion. The original capillary water pipes in the soil will be squeezed and blocked, reducing the permeability coefficient of the entire anti-seepage layer. The calcium sulfite hemihydrate in the desulfurization ash will also slowly oxidize over time to form calcium sulfate dihydrate, which will expand slightly in volume and absorb a certain amount of leachate, reducing the risk of leachate penetration.

[0058] The following describes embodiments of the present application. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application.

[0059] In the following examples and comparative examples, The red mud used is red mud produced by the Bayer process; Unless otherwise stated, the percentages mentioned are by mass; The moisture content of the mixture is based on the total mass of red mud and desulfurized ash; The percentage of carbide slag used is based on the total mass of desulfurization ash and red mud on a dry basis.

[0060] Example 1 The desulfurization ash used in this embodiment is dry desulfurization ash from a steel plant. The main components of the dry desulfurization ash are: 45.2% calcium sulfite, 21.7% calcium carbonate, and 22.3% calcium hydroxide.

[0061] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 52%; The main components of the red mud (on a dry basis) are: 28.6% aluminum oxide, 22.5% iron oxide, 23.5% silicon dioxide, and 21.1% calcium oxide; S2: Add desulfurized ash and red mud (on a dry basis) into a mixer at a mass ratio of 3:1 and stir for 10 minutes to obtain a mixture; The water content in the mixture is 27%, the mass ratio of calcium hydroxide to aluminum oxide is 3.3, and the mass ratio of calcium carbonate to aluminum oxide is 2.3; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to 76%, and the ball milling time is 40 minutes, so as to obtain an anti-seepage material containing CaAl type LDH.

[0062] Example 2 The desulfurization ash used in this embodiment is dry desulfurization ash from a steel plant. The main components of the dry desulfurization ash are: 42.2% calcium sulfite, 18.7% calcium carbonate, and 24.3% calcium hydroxide; The calcium hydroxide content of the carbide slag used is 80%.

[0063] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 45%; The main components of the red mud (on a dry basis) are: 24.6% aluminum oxide, 28.5% iron oxide, 30.5% silicon dioxide, and 11.1% calcium oxide.

[0064] S2: Add desulfurized ash, red mud (dry basis) and carbide slag (7%) into a mixer at a mass ratio of 2.5:1 and stir for 12 minutes to obtain a mixture; The water content in the mixture is 23%, the mass ratio of calcium hydroxide to aluminum oxide is 3.9, and the mass ratio of calcium carbonate to aluminum oxide is 1.9; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to be 80%, and the ball milling time is 60 minutes, so as to obtain an anti-seepage material containing CaAl type LDH.

[0065] Example 3 The desulfurization ash used in this embodiment is the dry desulfurization ash of a power plant. The main components of the dry desulfurization ash are: 30.2% calcium sulfite, 26.7% calcium carbonate, 13.3% calcium hydroxide, and the dust removal ash content in the desulfurization ash is 20.5%; The calcium hydroxide content of the carbide slag used is 85%.

[0066] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 44%; The main components of the red mud (on a dry basis) are: 18.6% aluminum oxide, 21.5% iron oxide, 38.5% silicon dioxide, and 16.1% calcium oxide.

[0067] S2: Add desulfurized ash, red mud (dry basis) and carbide slag (5%) into a mixer at a mass ratio of 2:1 and stir for 15 minutes to obtain a mixture; The moisture content in the mixture is 26%, the mass ratio of calcium hydroxide to aluminum oxide is 3.3, and the mass ratio of calcium carbonate to aluminum oxide is 2.9; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to be 88%, and the ball milling time is 80 minutes, so as to obtain an anti-seepage material containing CaAl type LDH.

[0068] Example 4 The desulfurization ash used in this embodiment is dry desulfurization ash from a steel plant. The main components of the dry desulfurization ash are: 39.7% calcium sulfite, 22.7% calcium carbonate, and 29.2% calcium hydroxide.

[0069] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 44%; The main components of the red mud (on a dry basis) are: 21.2% aluminum oxide, 27.3% iron oxide, 29.5% silicon dioxide, and 15.8% calcium oxide.

[0070] S2: Add desulfurized ash and red mud (on a dry basis) into a mixer at a mass ratio of 2.2:1 and stir for 10 minutes to obtain a mixture; The moisture content of the mixture is 25%, the mass ratio of calcium hydroxide to aluminum oxide is 4.0, and the mass ratio of calcium carbonate to aluminum oxide is 2.4; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to 78%, and the ball milling time is 50 minutes to obtain an anti-seepage material containing CaAl type LDH.

[0071] Example 5 The desulfurization ash used in this embodiment is dry desulfurization ash from a power plant. The main components of the dry desulfurization ash are: 25.2% calcium sulfite, 19.3% calcium carbonate, 17.4% calcium hydroxide, and the dust removal ash content in the desulfurization ash is 28.4%.

[0072] The calcium hydroxide content of the carbide slag used is 82%.

[0073] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 44%; The main components of the red mud (on a dry basis) are: 22.6% aluminum oxide, 25.4% iron oxide, 26.5% silicon dioxide, and 21.3% calcium oxide.

[0074] S2: Add desulfurized ash, red mud (dry basis) and carbide slag (addition amount is 4%) into a mixer at a mass ratio of 2.7:1 and stir for 14 minutes to obtain a mixture; The moisture content of the mixture is 21%, the mass ratio of calcium hydroxide to aluminum oxide is 3.9, and the mass ratio of calcium carbonate to aluminum oxide is 2.3; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to be 84%, and the ball milling time is 70 minutes, so as to obtain an anti-seepage material containing CaAl type LDH.

[0075] Example 6 The desulfurization ash in this example is dry desulfurization ash from a steel plant. The main components of the dry desulfurization ash are: 55.4% calcium sulfite, 26.3% calcium carbonate, and 14.4% calcium hydroxide; The calcium hydroxide content of the carbide slag used is 80%.

[0076] S1: sending the red mud slurry into a sedimentation tank for sedimentation to obtain sedimentation mud and supernatant, extracting the sedimentation mud into a dehydrator for dehydration to obtain red mud with a moisture content of 56%; The main components of the red mud (on a dry basis) are: 20.2% aluminum oxide, 31.8% iron oxide, 26.4% silicon dioxide, and 16.1% calcium oxide; S2: Add desulfurized ash, red mud (dry basis) and carbide slag (addition amount is 2%) into a mixer at a mass ratio of 2.7:1, and stir for 15 minutes to obtain a mixture; The moisture content of the mixture is 34%, the mass ratio of calcium hydroxide to aluminum oxide is 3.3, and the mass ratio of calcium carbonate to aluminum oxide is 3.5; S3: The mixed material is sent to a ball mill for ball milling to carry out a mechanochemical reaction, the ball milling speed is controlled to be 84%, and the ball milling time is 70 minutes, so as to obtain an anti-seepage material containing CaAl type LDH.

[0077] Example 7 The anti-seepage material was prepared according to the method of Example 1, except that the ball milling time was controlled to be 100 minutes.

[0078] Comparative Example 1 Natural clay was used as a comparison product.

[0079] Test Case The test examples are used to illustrate the anti-seepage performance of the anti-seepage materials of Examples 1-7 and the natural clay of Comparative Example 1.

[0080] 1. 1d, 7d permeability coefficient Samples were prepared and tested according to the test methods specified in Geotechnical Test Standard GB / T 50213-2019.

[0081] 2. 7d unconfined compressive strength The samples were prepared and measured according to the unconfined compressive strength test method specified in the Test Code for Inorganic Binder Stabilized Materials for Highway Engineering JTG E51-2024.

[0082] Table 1

[0083] Combined with the data in Table 1, it can be seen from the comparison between Examples 1-7 and Comparative Example 1 that the anti-seepage materials prepared in Examples 1-7 have 1d and 7d permeability coefficients comparable to or even lower than those of natural clay, indicating that the anti-seepage performance of the anti-seepage materials is comparable to or even better than that of natural clay. In addition, the anti-seepage materials of Examples 1-7 also have a relatively high 7d unconfined compressive strength, indicating that as time goes by, the anti-seepage materials will further react, thereby improving the anti-seepage effect and having a higher crack resistance.

[0084] In addition, by comparing Examples 1-5 with Example 6, it can be seen that controlling the water content of red mud at 44% to 52% is more conducive to improving the stability of LDH and improving the comprehensive performance of the anti-seepage material; by comparing Examples 1-5 with Example 7, it can be seen that controlling the ball milling time at 40 to 80 minutes can keep the anti-seepage material at an appropriate particle size while synthesizing LDH, avoiding excessive reaction and affecting the anti-seepage performance and later strength.

[0085] In summary, the anti-seepage material prepared in the present application is used as the anti-seepage layer material of the landfill. Due to the small fineness of the material, a hydration reaction will occur to generate calcium aluminate with a certain micro-expansion, which can close the capillary channels in the soil, thereby reducing the permeability coefficient of the system and providing a certain strength.

[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A method for preparing an anti-seepage material, characterized in that: The preparation method comprises: (1) mixing raw materials including red mud, desulfurization ash and optional additives to obtain a mixture; (2) subjecting the mixture to a ball milling mechanochemical reaction to form a layered calcium aluminum double hydroxide to obtain the anti-seepage material; wherein: The additive comprises calcium hydroxide, and the mass content of water in the red mud is 40% to 60%.

2. The preparation method according to claim 1, characterized in that: The preparation method further comprises: subjecting the red mud slurry to sedimentation and dehydration treatment to obtain the red mud.

3. The preparation method according to claim 1 or 2, characterized in that: The mass content of water in the red mud is 44% to 52%.

4. The preparation method according to any one of claims 1 to 3, characterized in that On a dry basis, the mass content of aluminum oxide in the red mud is 15% to 30%, and the mass content of silicon dioxide is 20% to 50%; Preferably, the mass content of calcium hydroxide in the desulfurized ash is 10% to 30%, the mass content of calcium carbonate is 10% to 30%, and the mass content of calcium sulfite is 25% to 60%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The mass ratio of the desulfurized ash to the red mud on a dry basis is (2-3):

1.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The additive is carbide slag, and the mass content of calcium hydroxide in the carbide slag is ≥80%; Preferably, the amount of the additive is 0-10% based on the total mass of the desulfurization ash and the red mud on a dry basis.

7. The preparation method according to any one of claims 1 to 6, characterized in that: In the mixture, the mass ratio of calcium hydroxide to aluminum oxide is (3-4):1, and the mass ratio of calcium carbonate to aluminum oxide is (0.5-5):1; Preferably, based on the total mass of the red mud and the desulfurization ash, the mass content of water in the mixture is 18% to 40%, more preferably 21% to 30%.

8. The preparation method according to any one of claims 1 to 7, characterized in that: In the ball milling mechanochemical reaction, the ball mill speed rate is 76% to 88%, and the ball milling time is 30 min to 100 min, preferably 40 min to 80 min.

9. An anti-seepage material obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the anti-seepage material according to claim 9 in a landfill anti-seepage system.