Method for recovering valuable components in hydrolysis mother liquor of titanium dioxide prepared by chlorination leaching method
Through step-by-step hydrolysis and multi-step reaction, the valuable components in the titanium hydrolysis mother liquor are recovered, and the problem of low recycling efficiency of valuable components in titanium dioxide production is solved, the added value and environmental protection of by-products are improved, and the efficiency of titanium dioxide is achieved. preparation.
Patent Information
- Application Number
- CN202411289422.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-14
AI Technical Summary
During the titanium dioxide production process, the recycling efficiency of the valuable components Ti, Ca, Cl, Fe, Al, Mn, Mg and Na in the titanium hydrolyzed mother liquor is low, resulting in low hydrochloric acid recovery rate, difficulty in handling solid waste, and long process flow, making it difficult to Realize industrialization.
Through step-by-step hydrolysis, spray roasting, absorption and evaporation, the valuable components in the titanium hydrolysis mother liquor, including iron oxide powder, manganese hydroxide, magnesium hydroxide and sodium chloride, were recovered separately, and the sulfuric acid, NaOH solution, etc. were used to perform the Multi-step reaction and filtration, control pH and temperature, and realize the precipitation and recovery of each metal ions.
It improves the recovery rate of valuable components in the titanium hydrolyzed mother liquor, produces high value-added by-products, reduces solid waste, enhances the environmental protection of the production process, and realizes the efficient preparation of titanium dioxide.
Smart Images

Figure CN118954615A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium dioxide production, and in particular to a green high value-added method for preparing titanium dioxide by chlorination leaching of titanium concentrate and titanium middlings. Background Art
[0002] Titanium dioxide refers to a white powder product with excellent pigment properties, the main chemical component of which is titanium dioxide (TiO2) and the particle size is 200-350nm. It is obtained by post-treatment with organic, inorganic or composite coatings. It is one of the most important inorganic chemical raw materials and is widely used in industrial fields such as coatings, plastics, papermaking, catalysis, rubber, ink, chemical fiber, and ceramics.
[0003] The wet process of titanium dioxide production technology includes sulfuric acid titanium dioxide production technology and hydrochloric acid (chlorination leaching) titanium dioxide production technology. Among them, sulfuric acid titanium dioxide production technology is a mature production technology with decades of production history, while chlorination leaching titanium dioxide production technology is being developed and beginning to be applied. The titanium raw material for the production of chlorination leaching titanium dioxide is mainly titanium concentrate. One of the methods for producing titanium dioxide is to decompose the titanium concentrate and iron powder with hydrochloric acid to obtain acid solution slurry. Titanium exists in the solution in the form of titanium oxychloride, and other impurities soluble in hydrochloric acid are decomposed into soluble chloride salts, mainly divalent iron salts, calcium salts, magnesium salts, manganese salts and trivalent aluminum salts. Undecomposed minerals are mixed in the solution in the form of solid impurities, which are removed by filtration, and the filtrate is then finely filtered to obtain titanium liquid. Titanium liquid is separated by freezing crystallization method to remove most of the ferrous iron from ferrous chloride tetrahydrate, concentrate the titanium liquid, hydrolyze the concentrated titanium liquid to prepare hydrated titanium dioxide, filter, wash, calcine, post-process and other processes to obtain pigment-grade titanium dioxide. The filtrate obtained after filtering the concentrated titanium liquid hydrolysis slurry is called titanium hydrolysis mother liquor. The currently available method is to prepare low-grade iron oxide powder that absorbs hydrochloric acid and contains oxides such as calcium, magnesium, manganese, and aluminum through spray roasting and absorption. The iron oxide powder has a high impurity content and is difficult to be used directly as an ironmaking raw material. Alternatively, the titanium hydrolysis mother liquor is treated by addition and subtraction neutralization precipitation method. The hydrochloric acid cannot be recovered, a large amount of waste slag is generated, and a large amount of waste salt solution is difficult to handle; the second method for producing titanium dioxide is to extract and separate the titanium liquid obtained by acid decomposition and filtration of titanium concentrate. 4+ and Fe 2+ , Fe 3+ , Ca 2+ Mg 2+ 、Al 3+The titanium dioxide is obtained by hydrolysis or spray heating hydrolysis, filtration and washing, drying, calcination and post-treatment of the refined titanium liquid. The typical process is the US ANI method (US6440383 and other patents), which takes the extraction of titanium as the first step. The Canadian CTL method (CA2513309 and other patents) takes the extraction of iron as the first step. There are also some literature reports on the effective separation of various metal elements from titanium. However, the stability of titanium liquid is low and the extraction efficiency is low, the separation effect of the extractant is poor, the process flow is long, the recovery rate of hydrochloric acid is low, and the solid waste and environmental protection problems have not been completely solved, making it difficult to achieve industrialization. Summary of the invention
[0004] The technical problem to be solved by the present invention is: to provide a method for separately recovering the valuable components contained in the titanium hydrolysis mother liquor in the production process of preparing titanium dioxide by the chlorination leaching method of titanium concentrate, which can utilize step-by-step hydrolysis, spray roasting, absorption and evaporation methods to separately recover the valuable components Ti, Ca, Cl, Fe, Al, Mn, Mg and Na contained in the titanium hydrolysis mother liquor, and the products can replace part of the production raw materials and serve as by-products, thereby increasing the added value of the products and making the process environmentally friendly.
[0005] The technical solution of the present invention is: a method for recovering valuable components in a hydrolysis mother liquor of titanium dioxide prepared by a chlorination leaching method, comprising the following steps:
[0006] (1) adding sulfuric acid to the hydrolysis mother liquor under stirring, heating and concentrating, condensing and recovering hydrochloric acid, and filtering after concentration to obtain a concentrated mother liquor and a perovskite composite material;
[0007] (2) heating the concentrated mother liquor of (1) obtained in the stirring step and introducing compressed air, adding NaOH solution, controlling the pH value to be less than or equal to 3, and conducting an oxidative hydrolysis reaction at 70-95° C., filtering after the reaction is completed to obtain an iron hydroxide filter cake and an iron precipitation filtrate, and spray roasting the iron hydroxide filter cake after dissolving to obtain iron oxide powder and recovering hydrochloric acid;
[0008] (3) heating and stirring the iron precipitation filtrate obtained in step (2), adding NaOH solution, controlling the pH value to be ≤4.2, and performing a hydrolysis reaction at 70-95° C., filtering after the hydrolysis is completed to obtain an aluminum hydroxide filter cake and an aluminum precipitation filtrate, and dissolving the aluminum hydroxide filter cake to produce a sodium tetrahydroxyaluminate solution;
[0009] (4) heating and stirring the aluminum precipitation filtrate obtained in step (3), adding NaOH solution, controlling the pH value to be ≤8.6, and performing a hydrolysis reaction at 70-95° C., filtering after the reaction is completed to obtain a manganese hydroxide filter cake and a manganese precipitation filtrate; the manganese hydroxide filter cake is dried and crushed to obtain a manganese hydroxide powder;
[0010] (5) heating and stirring the manganese precipitation filtrate obtained in step (4), adding NaOH solution, controlling the pH value to ≤ 10.7, and performing a hydrolysis reaction at 70-95° C., filtering after the hydrolysis is completed to obtain a magnesium hydroxide filter cake and a magnesium precipitation filtrate, and drying and crushing the magnesium hydroxide filter cake to obtain magnesium hydroxide powder;
[0011] (6) heating and evaporating the magnesium precipitation filtrate obtained in step (5) to crystallize sodium chloride, and centrifuging to obtain sodium chloride crystals.
[0012] Furthermore, in step (1), the added sulfuric acid reacts with the Ca 2+ The molar ratio is 1:1.
[0013] Furthermore, in step (2), the oxidative hydrolysis reaction time is 15-18 hours, and in steps (3), (4) and (5), the hydrolysis reaction time is 1.5-2 hours.
[0014] Furthermore, in step (4), the method for producing sodium tetrahydroxyaluminate solution after the aluminum hydroxide filter cake is dissolved is as follows: the aluminum hydroxide filter cake is stirred and slurried with water and heated to adjust the solid content to 20%, steam is introduced into the aluminum hydroxide slurry for heating, a 15% sodium hydroxide solution is added, stirred and dissolved to prepare a sodium tetrahydroxyaluminate solution for post-treatment of the aluminum coating of the primary titanium dioxide, the dissolution temperature is 40-60°C, the pH is controlled to be ≥12.5 during the process and at the end point, and the reaction time is 1-1.5 hours.
[0015] Furthermore, in step (6), the method for heating and evaporating the magnesium precipitation filtrate is as follows: the magnesium precipitation filtrate is pumped into a triple-effect evaporation system, triple-effect evaporation is performed using superheated steam, the sodium chloride crystal liquid reaching a supersaturated state is transported to a centrifugal separation device for separation to obtain sodium chloride crystals, and the filtrate is returned to the triple-effect evaporation system through a filtrate pump.
[0016] The present invention heats and concentrates the titanium hydrolysis mother liquor obtained by filtering the titanium liquid hydrolysis process to prepare hydrated titanium dioxide. 4+ Completely hydrolyze and add a certain amount of sulfuric acid to precipitate calcium ions in the form of calcium sulfate, condense and recover hydrochloric acid, and filter to obtain the perovskite composite material and concentrated mother liquor. 2+ Oxidized to Fe 3+ The valuable component Fe in the concentrated mother liquor was concentrated by step-by-step precipitation method with pH adjustment. 3+ 、Al 3+ , Mn 2+ Mg 2+The hydrolysis and precipitation are carried out in sequence. When the hydrolysis and precipitation of each element ion is complete and the other element ions have not yet been hydrolyzed and precipitated, the filtration and separation are carried out, and the filtrate is subjected to the hydrolysis and precipitation of the next element ion. The iron hydroxide filter cake obtained by filtering in the iron precipitation process is dissolved online in a plate and frame filter press using the leaching mother liquor produced in the preparation station of the porous silicon-titanium composite material in the previous process. The prepared ferric chloride solution is subjected to spray roasting and acid absorption processes to prepare iron oxide powder and iron salt roasting to absorb hydrochloric acid, and the absorbed hydrochloric acid is used as a leaching acid or analytical acid. The aluminum hydroxide filter cake is added with sodium hydroxide solution and stirred and dissolved to prepare a tetrahydroxyaluminate sodium solution for aluminum coating post-treatment, replacing the sodium aluminate raw material. The manganese hydroxide and magnesium hydroxide filter cakes are dried and crushed as by-products. The magnesium precipitation filtrate is a sodium chloride solution, and a sodium chloride product is prepared by triple-effect evaporation.
[0017] The titanium hydrolysis mother liquor is obtained by leaching titanium concentrate and titanium middlings with hydrochloric acid and HCl, filtering the leaching slurry, filtering the leaching liquid, freezing and crystallizing ferrous chloride and separating it, concentrating the clear titanium liquid, hydrolyzing the concentrated titanium liquid to prepare hydrated titanium dioxide, filtering and washing, and contains free hydrochloric acid, incompletely hydrolyzed Ti 4+ And dissolved chloride salts of Ca, Fe, Al, Mn, Mg, and Na. According to the calcium ion concentration in the hydrolysis mother liquor, Ca is added to the titanium hydrolysis mother liquor. 2+ / SO4 2- The molar ratio of 1:1 is a metered sulfuric acid solution. The titanium hydrolysis mother liquor is heated and concentrated in a concentration kettle. The mother liquor is concentrated to 12-18% of the original volume. The gas phase is condensed and absorbed to obtain condensed absorption acid. Ti 4+ Completely hydrolyzed to hydrated titanium dioxide, Ca 2+ The CaSO4 is precipitated and filtered to obtain the calcium titanium composite material and the concentrated mother liquor for iron precipitation. The calcium titanium composite material can be used as filler in the plastic, rubber and other industries after drying and calcination at 650±50℃.
[0018] The concentrated mother liquor of iron precipitation is heated and stirred in the iron precipitation reactor, and compressed air is introduced through the high-efficiency bubble distributor in the reactor. First, the oxygen in the compressed air is used to separate the Fe 2+ Partially oxidized to Fe 3+ :4FeCl2+O2+4HCl=4FeCl3+2H2O; the free HCl and Fe in the concentrated mother liquor 3+ Hydrolysis produces Fe 2+ The oxidation process requires the addition of excess HCl to neutralize and precipitate iron hydroxide with the addition of NaOH solution: FeCl3+3H2O=Fe(OH)3+3HCl, HCl+NaOH=NaCl+H2O. The hydrolysis temperature is 70-95℃, and the pH is controlled at ≤3 during the process and at the end point. 3+The metal ions other than the above are not hydrolyzed. After the hydrolysis is completed, the slurry is filtered in a modified plate-frame filter press, and the iron hydroxide filter cake is dissolved online in the plate-frame filter press with the leaching mother liquor. The leaching mother liquor used is the leaching mother liquor obtained by filtering and separating the porous silicon-titanium composite material prepared by the acid leaching residue of the titanium concentrate and the chlorination leaching with hydrochloric acid and HCl, which contains free acid and ferrous chloride. The ferric chloride solution for dissolving the iron hydroxide online is subjected to the spray roasting and acid absorption process to prepare iron oxide powder and iron salt roasting and absorption of hydrochloric acid.
[0019] The filtrate after iron precipitation is stirred and heated in the aluminum precipitation reactor. 3+ The HCl generated by hydrolysis is simultaneously added to the NaOH solution to neutralize and precipitate aluminum hydroxide. The hydrolysis temperature is 70-95°C, and the pH is controlled to be ≤4.2 during the process and at the end point. 3+ The metal ions other than the above are not hydrolyzed. The aluminum hydroxide filter cake and the filtrate after aluminum precipitation are obtained by filtration. The aluminum hydroxide filter cake is stirred and slurried by adding water in the aluminum dissolving reactor. The amphoteric properties of aluminum hydroxide are utilized to heat the aluminum dissolving reactor, stir and dissolve with sodium hydroxide solution to prepare the sodium tetrahydroxyaluminate solution for the post-treatment of the aluminum coating of the primary product of titanium dioxide. The dissolution temperature is 40-60°C, and the pH is controlled to be ≥12.5 during the process and at the end point.
[0020] The filtrate after aluminum precipitation is stirred and heated in the manganese precipitation reactor. 2+ The HCl generated by hydrolysis is simultaneously added to a NaOH solution to neutralize and precipitate manganese hydroxide. The hydrolysis temperature is 70-95°C, and the pH is controlled to be ≤8.6 during the process and at the end point. The manganese hydroxide filter cake and the filtrate after manganese precipitation are obtained by filtration. The manganese hydroxide filter cake is dried and crushed to obtain manganese hydroxide powder.
[0021] The filtrate after manganese precipitation is stirred and heated in the magnesium precipitation reactor. 2+ The HCl generated by hydrolysis is simultaneously added to a NaOH solution to neutralize and precipitate magnesium hydroxide. The hydrolysis temperature is 70-95°C, and the pH is controlled to be ≤10.7 during the process and at the end point. The hydrolysis slurry is filtered to obtain a magnesium hydroxide filter cake and a sodium chloride salt solution. The magnesium hydroxide filter cake is dried and crushed to obtain magnesium hydroxide powder.
[0022] The magnesium precipitation filtrate is crystallized into sodium chloride product through a triple-effect evaporator, and the evaporated condensed water is used in the production system.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention realizes the comprehensive utilization of vanadium-titanium magnetite resources, develops methods for respectively recovering the valuable components Ti, Ca, Cl, Fe, Al, Mn, Mg and Na contained in titanium hydrolysis mother liquor, and circularly recovers hydrochloric acid and aluminum compounds. The production process is environmentally friendly, and iron oxide powder, manganese hydroxide, magnesium hydroxide and sodium chloride by-products are produced, thereby increasing the added value of the products. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0026] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0027] Example 1
[0028] The contents of the components in the titanium hydrolysis mother liquor in this embodiment are:
[0029] Free HCl: 165.66 g / L, TiO2: 4.34 g / L, Fe 2+ :15.09g / L,Ca 2+ :2.18g / L,Al 3+ :1.18g / L,Mg 2+ :4.22g / L,Mn 2+ :1.33g / L,Na + :1.67g / L, total Cl - :206.01g / L.
[0030] The titanium hydrolysis mother liquor from the titanium hydrolysis mother liquor storage tank is metered into the hydrolysis mother liquor concentration reactor by the mother liquor feed pump, and the feed amount is 17.41m 3 / hr, start stirring and add 70% mass concentration sulfuric acid, the feed rate is 74L / hr. Turn on the steam, use the jacket indirect heat exchange method to heat the titanium hydrolysis mother liquor to boiling, condense and recover the hydrolysis mother liquor condensed acid, about 14.70m 3 / hr, pumped to the hydrated titanium dioxide secondary wash acid storage tank, the free HCl concentration is: 192.68g / L, used for hydrated titanium dioxide filter cake washing.
[0031] The concentrated mother liquor flows into the concentrated mother liquor storage tank, and the discharge volume is 2.68m 3 / hr. The concentrated mother liquor in the concentrated mother liquor storage tank is pumped to the diaphragm filter press for filtration, and the filtrate is pumped to the iron precipitation liquid storage tank. The filter residue is a calcium titanium composite material, which can be used as a filler in the plastic, rubber and other industries after drying and calcination at 650±50℃. The content of each component in the concentrated mother liquor clear liquid is: free HCl: 15.51g / L, Fe 2+ :98.05g / L,Al 3+ :7.67g / L,Mg 2+ :27.45g / L,Mn 2+ :8.62g / L,Na + :10.64g / L, total Cl - :272.37g / L.
[0032] The 2.6m3 of iron precipitate in the storage tank 3 The concentrated mother liquor for iron precipitation is pumped into the iron precipitation reactor, stirred and heated, and compressed air is introduced through the high-efficiency bubble distributor in the reactor. First, the oxygen in the compressed air is used to precipitate Fe under the acidic conditions of the concentrated mother liquor itself. 2+ Partially oxidized to Fe 3+ , free HCl and Fe 3+ Hydrolysis produces Fe 2+ The excess HCl in the oxidation process is simultaneously added with 15% NaOH solution to neutralize and precipitate iron hydroxide. The hydrolysis temperature is 70-95°C, the oxidation-hydrolysis reaction time is 15-18 hours, and the pH is controlled at ≤3 during the process and at the end point. 3+ Other metal ions are not hydrolyzed.
[0033] After the hydrolysis is completed, the slurry is pumped to the modified plate and frame filter press for filtration. The filtrate is pumped to the aluminum precipitation liquid storage tank, about 2.75m 3 The content of each component in the aluminum precipitation liquid is: Al 3+ :7.42g / L,Mg 2+ :26.62g / L,Mn 2+ :8.28g / L,Na + :101.39g / L, total Cl - :269.27g / L.
[0034] The iron hydroxide filter cake is dissolved online in a plate-frame filter press with a leaching mother liquor. The leaching mother liquor used is the leaching mother liquor obtained by filtering and separating the porous silicon-titanium composite prepared by acid leaching residue of titanium concentrate with hydrochloric acid and HCl chlorination. The composition of the leaching mother liquor is as follows: free HCl: 156.49 g / L, Fe 2+ : 88.35g / L, the amount of leaching mother liquor used is 2.43m 3 The acidic ferric chloride solution obtained by dissolving ferric hydroxide online is pumped to the ferric chloride solution intermediate storage tank.
[0035] The outlet valve of the intermediate storage tank of ferric chloride solution was opened, and the ferric chloride solution was sprayed into the roasting furnace, contacted with hot air at a temperature of 750-850°C, and reacted with O2 and H2O to decompose into H2O+HCl mixed gas+ferric oxide powder. The storage tank for absorption acid was opened, and the washing acid after washing the hydrated titanium dioxide filter cake was used as the absorption liquid of the falling film absorption system in the spray roasting section to produce regenerated acid, which was pumped into the regenerated acid storage tank for chlorination leaching. The regenerated acid concentration was 348.32g / L. 718.48kg of ferric oxide powder was obtained.
[0036] The 2.75m3 aluminum precipitate storage tank 3 After iron precipitation, the filtrate is pumped into a volume of 4m3 The aluminum precipitation reactor is stirred and heated by steam jacket. 3+ The HCl generated by hydrolysis is simultaneously added with 15% NaOH solution to neutralize and precipitate aluminum hydroxide. The hydrolysis temperature is 70-95°C, the hydrolysis reaction time is 1.5-2 hours, and the pH is controlled to be ≤4.2 during the process and at the end point. 3+ Other metal ions are not hydrolyzed.
[0037] Al 3+ After the hydrolysis is completed, the aluminum slurry is pumped to the plate and frame filter press for filtration. The filtrate is pumped to the manganese precipitate storage tank, about 2.8m 3 The content of each component in the manganese precipitation solution is: Mg 2+ :26.12g / L,Mn 2+ :8.24g / L,Na + :120.35g / L, total Cl - :268.25g / L.
[0038] The aluminum hydroxide filter cake obtained by filtration and washing is shoveled into a 2m 3 The aluminum hydroxide filter cake obtained from the multiple reaction processes is stirred and slurried with water and heated to adjust the solid content to 20%. The steam valve is opened to pass steam into the aluminum hydroxide slurry for heating, the sodium hydroxide feed pump is turned on, and a 15% sodium hydroxide solution is added, stirred and dissolved to prepare a sodium tetrahydroxyaluminate solution for post-treatment of the aluminum coating of the primary titanium dioxide, the dissolution temperature is 40-60°C, the pH is controlled to be ≥12.5 during the process and at the end point, and the reaction time is 1-1.5 hours.
[0039] Open the manganese precipitation liquid storage tank and pour 2.8m 3 After aluminum precipitation, the filtrate is pumped into a volume of 4m 3 In the manganese precipitation reactor, start stirring, open the steam regulating valve to heat the steam jacket, Mn 2+ The HCl generated by hydrolysis is simultaneously added with a 15% NaOH solution to neutralize and precipitate manganese hydroxide. The hydrolysis temperature is 70-95° C., the pH is controlled to be ≤8.6 during the process and at the end point, and the hydrolysis reaction time is 1.5-2 hours.
[0040] Mn 2+ After the hydrolysis is completed, the manganese slurry is pumped to the plate and frame filter press for filtration. The filtrate is pumped to the magnesium precipitate storage tank, about 2.82m 3 The content of each component in the manganese precipitation solution is: Mg 2+ :26.08g / L,Na + :126.43g / L, total Cl - :266.43g / L.
[0041] The manganese hydroxide filter cake obtained by filtering and washing is dried and crushed to obtain manganese hydroxide powder.
[0042] 2.82m3 of manganese precipitation solution in the storage tank 3 After manganese precipitation, the filtrate is pumped into a volume of 4m 3 In the magnesium precipitation reactor, start stirring, open the steam regulating valve to heat the steam jacket, Mg 2+ The HCl generated by hydrolysis is simultaneously added with 8% NaOH solution to neutralize and precipitate magnesium hydroxide. The hydrolysis temperature is 70-95° C., the pH is controlled to be ≤10.7 during the process and at the end point, and the hydrolysis reaction time is 1.5-2 hours.
[0043] Mg 2+ After the hydrolysis is completed, the magnesium slurry is pumped to the plate and frame filter press for filtration and washing. The filtrate is pumped to the sodium chloride liquid storage tank, about 3.55m 3 The content of each component in the magnesium precipitation solution is: Na + :140.12g / L,Cl - :211.73g / L.
[0044] The magnesium hydroxide filter cake is filtered and washed, and then dried and crushed to obtain magnesium hydroxide powder.
[0045] The brine from the sodium chloride liquid storage tank is metered and pumped into the triple-effect evaporation system by the brine feed pump, and triple-effect evaporation is performed using superheated steam. The supersaturated sodium chloride crystal liquid is transported to the centrifugal separation equipment for separation, and the filtrate is returned to the triple-effect evaporation system through the filtrate pump. The water content of the separated sodium chloride crystals is 3-5%.
Claims
1. A method for recovering valuable components from the hydrolysis mother liquor of titanium dioxide prepared by chlorination leaching, characterized in that: The steps include: (1) adding sulfuric acid to the hydrolysis mother liquor under stirring, heating and concentrating, condensing and recovering hydrochloric acid, and filtering after concentration to obtain a concentrated mother liquor and a perovskite composite material; (2) heating the concentrated mother liquor of (1) obtained in the stirring step and introducing compressed air, adding NaOH solution, controlling the pH value to be less than or equal to 3, and conducting an oxidative hydrolysis reaction at 70-95° C., filtering after the reaction is completed to obtain an iron hydroxide filter cake and an iron precipitation filtrate, and spray roasting the iron hydroxide filter cake after dissolving to obtain iron oxide powder and recovering hydrochloric acid; (3) heating and stirring the iron precipitation filtrate obtained in step (2), adding NaOH solution, controlling the pH value to be ≤4.2, and performing a hydrolysis reaction at 70-95° C., filtering after the hydrolysis is completed to obtain an aluminum hydroxide filter cake and an aluminum precipitation filtrate, and dissolving the aluminum hydroxide filter cake to produce a sodium tetrahydroxyaluminate solution; (4) heating and stirring the aluminum precipitation filtrate obtained in step (3), adding NaOH solution, controlling the pH value to be ≤8.6, and performing a hydrolysis reaction at 70-95° C., filtering after the reaction is completed to obtain a manganese hydroxide filter cake and a manganese precipitation filtrate; the manganese hydroxide filter cake is dried and crushed to obtain a manganese hydroxide powder; (5) heating and stirring the manganese precipitation filtrate obtained in step (4), adding NaOH solution, controlling the pH value to ≤ 10.7, and performing a hydrolysis reaction at 70-95° C., filtering after the hydrolysis is completed to obtain a magnesium hydroxide filter cake and a magnesium precipitation filtrate, and drying and crushing the magnesium hydroxide filter cake to obtain magnesium hydroxide powder; (6) heating and evaporating the magnesium precipitation filtrate obtained in step (5) to crystallize sodium chloride, and centrifuging to obtain sodium chloride crystals.
2. The method according to claim 1, characterized in that In step (1), the added sulfuric acid reacts with the Ca in the hydrolysis mother liquor. 2 + The molar ratio is 1:
1.
3. The method according to claim 1, characterized in that In step (2), the oxidative hydrolysis reaction time is 15-18 hours, and in steps (3), (4) and (5), the hydrolysis reaction time is 1.5-2 hours.
4. The method according to claim 1, characterized in that: In step (4), the method for producing sodium tetrahydroxyaluminate solution after the aluminum hydroxide filter cake is dissolved is as follows: the aluminum hydroxide filter cake is stirred and slurried with water and heated to adjust the solid content to 20%, steam is introduced into the aluminum hydroxide slurry for heating, a 15% sodium hydroxide solution is added, stirred and dissolved to prepare a sodium tetrahydroxyaluminate solution for post-treatment of aluminum coating of titanium dioxide primary product, the dissolution temperature is 40-60°C, the pH is controlled to be ≥12.5 during the process and at the end point, and the reaction time is 1-1.5 hours.
5. The method according to claim 1, characterized in that In step (6), the method for heating and evaporating the magnesium precipitation filtrate is as follows: the magnesium precipitation filtrate is pumped into a triple-effect evaporation system, triple-effect evaporation is performed using superheated steam, the sodium chloride crystal liquid reaching a supersaturated state is transported to a centrifugal separation device for separation to obtain sodium chloride crystals, and the filtrate is returned to the triple-effect evaporation system through a filtrate pump.
Citation Information
Patent Citations
Method of preparing ferric vanadate from residue of aluminum powder vanadium removal of crude titanium tetrachloride
CN104649328A
Process for preparing calcium chloride by utilizing titanium dioxide byproduct hydrochloric acid residue water
CN112520777A
Titanium dioxide chlorination dust collection slag iron resource recovery process
CN115536073A
Water resource treatment system for collecting dust and waste residues of titanium dioxide prepared by chlorination method
CN214115239U
Process for recovering vanadium values from acidic chloride solutions
US4150092A