Method for preparing concrete for slip form construction by adding attapulgite-based thixotropic agent
Through acid activation and surface micro-hydrophobic treatment of Mingguang Concave and concave rock stones, combined with composite admixtures, concrete that meets the requirements of sliding form construction is prepared, which solves the problems of concrete flowability and compactness in sliding form construction, and improves construction efficiency and safety sex.
Patent Information
- Application Number
- CN202411122583.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
In sliding form construction, concrete mixture is difficult to meet the requirements of fluidity, viscosity and compactness during transportation and paving, resulting in low construction efficiency, poor quality and safety hazards, and the existing concave and concave rock stone technology is not fully utilized. Its structural characteristics and physical and chemical properties.
The acid activation and surface micro-hydrophobic treatment was used to prepare a thixotropic slurry, and mixed with the optimized proportional compound admixture and other raw materials to form excellent slump, compactness and strength. concrete for sliding form construction.
It realizes high flowability, rapid condensation and high strength of concrete in sliding form construction, meets construction speed and quality requirements, reduces transportation and paving difficulties, and improves construction efficiency and safety.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing concrete for sliding film construction, in particular to a method for preparing concrete for sliding film construction by adding an attapulgite-based thixotropic agent, and belongs to the field of green and low-carbon building materials. Background Art
[0002] With the rapid development of my country's social economy and science and technology, the structure of infrastructure projects has become more complex and developed in a multi-dimensional direction. The construction technology has gradually developed towards mechanization, intelligence and integration. The construction industry has also paid more attention to technological innovation to drive quality improvement, efficiency improvement and high-quality development. Slipform construction is a construction technology for cast-in-place concrete projects. The use of a slipform paver will compact and pave the freshly mixed concrete transported to the construction site in one go. It can be called a "3D printer for cement concrete" and is highly favored by all walks of life. Slipform construction has the advantages of high degree of mechanization, fast construction speed, good structural integrity, high surface finish, beautiful and straight lines. Compared with the traditional process of manual formwork, it has incomparable advantages in reducing labor intensity, reducing material consumption, improving construction quality and efficiency, ensuring safe operations, and improving comprehensive benefits.
[0003] Slipform paving has been demonstrated in the construction of concrete pavements, roads, bridge guardrails, curbstones, slopes, ditches and other ancillary structures. However, with the promotion and application of this technology, the quality of concrete products and technical problems on the construction site have also arisen. For example, when slipform construction is used to pave concrete anti-collision guardrails with a certain vertical height (about 1.2m), the workability of the concrete mixture is required to be high, and it should have the characteristics of low slump, high cohesion, early strength and fast hardening, and rapid forming. Moreover, as a small-sized component of roads and bridges, the concrete guardrail has a long longitudinal continuous length. The appearance quality of the component must be strictly controlled to meet the principles of solid inside and bright outside, accurate size, linear straightness, and consistent color. However, in the process of guardrail slipform paving, in order to facilitate construction, dry hard concrete (slump should be controlled at 30±10mm) is often used. Too small slump makes it difficult for concrete to enter and exit the tank of the mixer truck, and it is easy to stick to the tank during transportation, making it difficult to transport with a concrete mixer truck. It can only be transported to the site by a tank truck and then spread by an excavator, which greatly increases the difficulty and cost of concrete transportation and spreading. In addition, due to insufficient vibration liquefaction during the paving process, voids will form in the lower part of the guardrail, and even the newly laid concrete guardrail will sink. Choosing concrete with too large a slump will cause poor cohesion, pockmarked segregation, linear distortion, early cracking and shrinkage, etc. The working performance, strength after hardening and durability of the concrete will be reduced, which will pose a safety hazard to traffic safety and increase the economic cost of subsequent maintenance and repair.
[0004] During the entire slipform construction process, the concrete mixture must not only have good fluidity, wrapping and water retention during transportation and spreading, but also have good cohesion, compactness and shape retention during vibration, extrusion and paving. On the premise that the slipform construction equipment is quite mature, the technical difficulty of the slipform construction process lies in the design of the mix ratio of the concrete mixture, the regulation of working properties such as workability and thixotropy. Only when the slipform construction concrete has excellent working properties (such as workability, compactness, strength and stability) to meet the construction requirements of each stage of slipform construction, and cooperate with the smooth operation of the slipform paver, can the high quality and high efficiency of the slipform construction process be fully demonstrated. At the same time, appropriate admixtures should be selected according to the transportation distance, environment, climate and other conditions to ensure and improve the working performance of concrete mixtures. The water reduction rate of a single polycarboxylic acid high-performance water-reducing agent is high, which makes the concrete have a high fluidity, but the plasticity is poor, which seriously affects the construction progress and quality of slipform construction. This requires the optimization of functional components with good compatibility and green environmental protection to obtain a composite admixture to improve the workability and shape retention of concrete. Therefore, it is of great practical significance to prepare a slipform construction concrete that can meet the working performance requirements of slipform construction and has good plasticity and high early strength.
[0005] In the construction industry, the working performance of cementitious materials is often improved by adding chemical modifiers (such as hydroxyethyl cellulose ether, hydroxypropyl methyl cellulose ether) or polymer additives. Unlike chemical additives, natural micro-nanostructured clay minerals have excellent surface effects, volume effects, size effects, and filling effects, and have become the first choice for environmentally friendly functional materials and new auxiliary fillers. Among them, attapulgite is a hydrated magnesium-aluminum silicate clay mineral with a layered chain structure. It is a natural one-dimensional nanostructured material. Its unique nanorod-like crystal morphology, pore structure, and charged properties give it excellent colloidal properties, adsorption properties, and reinforcement and toughening properties for polymer materials. It is widely used in various industrial fields such as petroleum, chemical industry, environmental protection, medicine, food, and energy. Studies have shown that green, environmentally friendly and low-cost attapulgite can improve the working performance and application performance of concrete materials. For example, attapulgite can be used to prepare thixotropic agents for slipform concrete of bridge piers, attapulgite and other clay minerals can be used to prepare thickeners for concrete, attapulgite can be used as a concrete component to improve concrete strength, or attapulgite can be used to improve the thermal insulation performance of concrete blocks. Patents such as a slipform concrete for high piers of highway bridges and a preparation method thereof (CN118221399A), an ultra-high performance concrete composition that can be sprayed for construction (CN114075059A), a cementitious material containing modified basalt fiber and a preparation method thereof (CN113173749B), a nanoporous concrete with a thixotropic colloid as a template and a preparation method thereof (CN105294141A), a concrete composite admixture and a preparation method thereof (CN113292273A), a concrete and a preparation method thereof (CN107879690 A), a preparation method of nano-attapulgite recycled concrete (CN113773016A), and a red mud / attapulgite ceramsite concrete hollow insulation block and a preparation method thereof (CN103253907B) all involve this content. However, the above-mentioned technical solutions for using attapulgite to improve the working performance of concrete only utilize the viscosity of attapulgite, the activity of attapulgite calcined at high temperature, or the use of attapulgite to surface-modify basalt fiber to increase surface activity and other technical characteristics, and fail to achieve truly efficient utilization of attapulgite's own unique structural characteristics, physical and chemical properties and micro-nano effects.
[0006] In fact, not all attapulgite has viscosity-increasing and thixotropic properties at low concentrations. Only the Mingguang attapulgite with relatively complete development, high purity, large rod crystal length / diameter ratio and trioctahedral crystal structure has excellent viscosity-increasing and thixotropic properties. Increasing the amount of attapulgite added will inevitably increase the viscosity and thixotropy of the suspension. Exceeding a certain amount (such as ≥2%) will make the concrete mixture instantly dry and hard, lose fluidity, and cause great trouble to subsequent construction. At the same time, in view of the particularity of the slipform construction process and the high requirements for the working performance of the concrete used, it is also necessary to pay attention to the selection and quality control of the raw materials of concrete for slipform construction, the design of the mix ratio, the compounding of functional admixtures and the mixing process and other key control factors, which are of great practical significance for the promotion and application of slipform construction technology in the construction industry. Based on this, the present invention quantitatively analyzes the structure-activity relationship between key factors such as the amount of attapulgite thixotropic agent added, the proportion of key functional components in the composite admixture, the mix ratio and the working performance of the concrete mixture through multiple strategies such as adding Mingguang attapulgite thixotropic agent slurry, regulating the functional components and proportions in the composite admixture, optimizing the mix ratio and mixing in steps, and successfully prepares concrete with excellent slump retention, compactness, workability and strength, which has good application prospects in slipform construction, 3D printing, complex component manufacturing and other fields. Summary of the invention
[0007] In view of the fact that the above-mentioned concrete mixture cannot simultaneously meet the specific working performance requirements in the transportation, distribution, paving and molding stages of the sliding film construction, which seriously limits the full play of the advantages of the sliding film construction process in terms of construction speed, construction quality, and comprehensive economic benefits, the present invention provides a method for preparing concrete for sliding film construction by adding a attapulgite-based thixotropic agent based on a deep understanding of the sliding film construction process, the specific working performance requirements of concrete for sliding film construction, and the physical and chemical properties of Mingguang attapulgite. First, the Mingguang attapulgite is acid-activated and surface-micro-hydrophobicized to obtain a thixotropic agent slurry, and then materials such as cement, fly ash, sand, crushed stone, water, composite admixture (formed by compounding polycarboxylic acid water reducer, sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate) and the thixotropic agent slurry with optimized ratios are added and mixed step by step to obtain concrete for sliding film construction.
[0008] The method for preparing concrete for sliding film construction by adding attapulgite-based thixotropic agent of the present invention is characterized in that the concrete is mixed with the following raw materials in parts by weight: 315-320 parts of cement, 55-60 parts of fly ash, 840-850 parts of sand (mud content ≤1.0%), 305-315 parts of crushed stone (5-10 mm), 720-725 parts of crushed stone (10-20 mm), 180-190 parts of water, 5-6 parts of composite admixture, 1.5-3.0 parts of attapulgite-based thixotropic agent. The cement is any one or more of silicate cement, white cement and sulphoaluminate cement, the dosage of desulfurized gypsum and alcohol amine grinding aid is ≤6% and 0.1% respectively; the fly ash is F-grade fly ash, the water requirement ratio (%) is ≤90; the mud content in the crushed stone is ≤1.0%. The sand is natural sand or washed sand, mainly medium-coarse sand, with a fineness modulus of 2.6 to 3.2, wherein the flocculant content in the washed sand is ≤0.5%. The composite admixture is a C6 polycarboxylic acid water reducer (water reduction rate is 25 to 35%) and sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate (AOS) mixed and compounded at a mass ratio of 100:2 to 4:2 to 3:1 to 2:0.25 to 1.0. The design of the above mix ratio is based on the basic technical properties of the raw materials and the specific conditions of the slipform construction, combined with the preliminary mix ratio design of concrete and the laboratory mix ratio test, and systematically examines the influence of the water-binder ratio, unit water consumption, sand ratio, admixture components and the changes in the amount of addition on the workability, slump and mechanical strength of the concrete. The amount of the component materials that can meet the construction conditions, mechanical properties and other technical and economic indicators required by the slipform construction is finally determined.
[0009] Among them, if the mud content in the fine aggregate sand is too large, the mud minerals therein will absorb the functional components in the composite admixture, greatly reducing the efficacy of the composite admixture and the synergistic enhancement effect between the components, and even causing the admixture to fail. Therefore, the mud content in the sand needs to be controlled to ≤1.0%; at the same time, the particle shape and surface characteristics of the sand will affect its bonding with cement and the fluidity of the concrete mixture. In order to meet the fluidity of concrete in slipform construction, it is preferred to use medium-coarse sand as the main material with a fineness modulus of 2.6 to 3.2, and fill the gaps between the coarse sand with an appropriate amount of medium-sized sand. The total void ratio and total surface area are reduced, which not only reduces the amount of cement slurry used, but also improves the density and strength of the concrete; and if washed sand is used, the flocculant content in the washed sand needs to be limited to ≤0.5%. This is because the trace flocculant contained in the sand will reduce the strength of the concrete, resulting in damage to the shape retention of the concrete during the slipform construction process. In addition, the maximum particle size of coarse aggregate is limited by the structural type and the density of reinforcement. The surface condition of coarse aggregate is also closely related to strength. Considering that the feeding is completed by the spiral distributor during the slipform construction process, and the concrete passes through the tied steel mesh and tightly wraps the steel bars during the paving process, the maximum particle size of the crushed stone in the aggregate is optimized and controlled. The crushed stone with two particle sizes of 5-10mm and 10-20mm is selected and applied according to the mass ratio of 3:7, which not only ensures the operability of feeding and paving during the slipform construction process, but also satisfies the requirements that the slipform construction concrete has sufficient strength and smooth surface. At the same time, in order to meet the requirements that the slipform construction concrete must have both fluidity (transportation process) and rapid cohesion and formwork (paving), the technical characteristics such as the dosage of desulfurized gypsum and alcohol amine grinding aids in cement and the water demand ratio of fly ash are also limited to ensure that the concrete used for slipform construction has excellent working performance.
[0010] The preparation method of the attapulgite-based thixotropic agent is as follows: after pulping acid activation and surface micro-hydrophobic treatment, the Mingguang attapulgite ore is dispersed in water with a solid content of 5-7% and stirred for hydration for at least 12 hours to obtain a thixotropic agent slurry, and added in the form of slurry. The attapulgite content in the Mingguang attapulgite ore is ≥75%, and the mass fraction of MgO in the chemical composition tested by XRF is 10-14%. The pulping acid activation is to crush the Mingguang attapulgite ore into 100 meshes, ultrasonically disperse it in a sulfuric acid or phosphoric acid aqueous solution with a pH value of 3.5-4.0, and stir and react for 4-8 hours. The surface micro-hydrophobic treatment process is as follows: first, oleic acid glyceride or silane coupling agent is added to an alcohol-water mixed solution (alcohol / water volume ratio=8:2) to obtain a uniform modified solution; then, acid-activated attapulgite is ultrasonically dispersed into the above-mentioned modified solution with a solid content of 7%, heated (80-90°C) and refluxed with stirring for 6-8h, and then centrifuged and dried to obtain a surface micro-hydrophobic treated powder, wherein the amount of oleic acid glyceride or silane coupling agent added is 0.5-2.0% of the mass of the acid-activated attapulgite.
[0011] From the physicochemical properties of different attapulgite (Table 1) and SEM images ( Figure 1 ) comparison shows that the Mingguang attapulgite with a trioctahedral rod crystal structure has the characteristics of high purity, large rod crystal length / diameter ratio, high MgO content, large specific surface area and pore volume. Under the same processing conditions (7% solid content, stirring at 11000rpm for 20 minutes), the initial viscosity of the Mingguang attapulgite suspension is 20 and 100 times that of the Xuyi attapulgite and Linze mixed-fiber attapulgite clay suspensions, respectively. At a low addition amount (2%), there is almost no sedimentation within 2 hours, and it exhibits extremely excellent suspension stability, which is attributed to the unique properties of Mingguang attapulgite such as high purity, long rod crystals and crystal structure. At the same time, the unique structural characteristics and physical and chemical properties are conducive to the entanglement and interlacing of the nanorod crystals and rod crystal bundles of Mingguang attapulgite in a static state to form flocculated aggregates, which bind a large number of water molecules in the network structure to form a gel with low fluidity and high bearing capacity. After repeated shearing or stirring, the three-dimensional network structure formed is destroyed, and the release of water molecules in it will increase the fluidity of the composite, which is conducive to showing the thixotropic characteristics of concrete that are crucial in sliding film construction. The rheological properties of cement paste were tested using a rheometer (Anton-Paar MCR102), and the ratio of its initial stress / equilibrium stress was defined as the thixotropic index, which can quantitatively describe the relationship between static and dynamic yield stresses. The larger the thixotropic index, the easier it is for the composite cement paste material to thicken statically and thin by shear, and the better the thixotropic property of the composite cement paste. The above three types of attapulgite were dispersed at a high speed in cement paste at a mass fraction of 0.5%. It was found that the thixotropy index of the neat cement paste was only 1.93, while the addition of Mingguang attapulgite had the greatest improvement on the thixotropy index of the neat cement paste (about 25%), which confirmed that the addition of Mingguang attapulgite makes it easier to obtain cement-based cementitious materials with low dynamic yield stress, high static yield stress and thixotropy, which makes it have good development potential in thixotropic concrete application fields such as sliding film construction and 3D printing.
[0012] This application selects Mingguang attapulgite with long rod crystals, high viscosity and thixotropy to prepare the thixotropic agent of concrete, and adds it in the form of hydrated slurry (reducing the influence of body water absorption on the water-binder ratio of concrete), which will not affect its compatibility with other concrete substrates, and can give full play to the nanocrystalline structure and colloidal properties of Mingguang attapulgite. At the same time, the adsorption performance of Mingguang attapulgite is not as good as the other two types of attapulgite. When added to the concrete mixture, its adsorption capacity for functional components such as water reducer and air entraining agent is weak, which is more conducive to the functional components to play the corresponding effect. Among them, Mingguang attapulgite can remove unstable carbonates, soluble salts and other impurities in the original ore after acid activation, and the conductivity value of the acid-activated slurry is significantly reduced, which proves that the number of soluble salts is reduced, and the sparse pore structure is also conducive to the combination with the micro-hydrophobic modifier; and the pH value of the acid-activated solution is limited to 3.5-4.0 to prevent the viscosity of attapulgite from being greatly reduced during the acidification process, affecting the actual application performance in slipform construction. The acid-activated attapulgite is then treated with surface micro-hydrophobicity. On the one hand, it can weaken the strong adsorption of attapulgite on free water and free water in the concrete system, so that there is sufficient water in the system for hydration, hydration and lubrication. On the other hand, it can turn attapulgite into an amphiphilic, highly dispersible thixotropic agent. One end of the mineral is hydrophilic, and the other end of the grafted long-chain organic molecule can not only disperse the attapulgite-based thixotropic agent evenly in the gap between the cement paste and the aggregate through electrostatic repulsion, but also combine with the free components in the composite admixture to improve the thixotropic and water retention properties. Finally, after the Mingguang attapulgite after acid activation and surface micro-hydrophobicity treatment is fully hydrated, it is added to the concrete in the form of thixotropic agent slurry, which solves the problem that the attapulgite has strong hydrophilicity and causes the concrete mixture to dry and harden quickly, and does not have the fluidity requirements for slipform construction and transportation. At the same time, the highly dispersible thixotropic agent slurry can quickly disperse and act between inorganic-organic materials, and exhibit excellent thixotropy, filling effect and toughening and reinforcement effect during vibration and paving.
[0013] The composite admixture is prepared by adding optimized proportions of retarder, collapse preventer, air entraining agent and defoamer to high-efficiency C6 polycarboxylic acid water reducer. The concrete mixing process is as follows: first, add 80% of water and composite admixture to the evenly mixed cement, sand, crushed stone and fly ash dry materials and stir for 2 to 3 minutes, then add attapulgite-based thixotropic agent slurry and stir again for 2 to 3 minutes to obtain concrete for slipform construction. Slump, compactness and strength are the key technical indicators for measuring the working performance and quality control of concrete mixtures for slipform construction. Among them, the initial slump and the change of slump over time intuitively reflect the workability, self-compacting and shape retention ability of concrete, and high-strength concrete can not only ensure the quality of construction projects, but also provide strong protection for building safety. From the change of slump of the prepared concrete over time ( Figure 2) It can be seen that in Comparative Example 1, the mix ratio used in the on-site formwork casting method is used. Slight bleeding will occur in the prepared concrete mixture. The slump becomes 30mm after 1 hour. There are some small depressions on the surface of the concrete specimen. The fluidity and self-compactness of the concrete are poor and cannot meet the requirements of slipform construction concrete. Comparative Example 2 is to add Mingguang attapulgite (0.5% of the mass of cementitious material) slurry under the same mix ratio. The workability of the concrete mixture is significantly improved. Although the slump loss is large after 1 hour and still cannot meet the construction requirements of slipform construction concrete, the surface of the concrete specimen after collapse is smoother and denser, indicating that the addition of attapulgite can significantly improve the workability and compactness of the concrete. Further, from the time-dependent changes in the slump of the concrete of Examples 1 to 3 ( Figure 2 ) It can be clearly seen that the concrete mixtures added with the slightly hydrophobized Mingguang attapulgite thixotropic agent slurry and the composite admixture did not show rapid cohesion or dry hardening, but always showed excellent workability, cohesion and shape retention within 2 hours, and the slump was maintained between 130 and 190 mm. The cement slurry and aggregate had good encapsulation. In particular, the stacking morphology of the concrete specimens after collapse in Example 3 was approximately an ideal truncated cone, and the surface of the specimens was smoother, denser, and had no collapse. It had excellent thixotropy and self-compacting ability, and could fully meet the working performance requirements of slipform construction concrete.
[0014] CT scanning technology is an innovative, non-destructive way to deeply study the microstructure of concrete, which can better reflect the spatial distribution of aggregates and pores in concrete and the characteristics of pore structure. In addition, due to the different densities of cement mortar and stone materials in concrete and the pores inside, the absorption coefficient of concrete to X-rays is different, that is, the CT value is different. The size of the CT value directly reflects the density and compactness of the concrete material. The larger the CT value, the denser and more compact the concrete material is, and the corresponding mechanical strength is also greater. From the CT scanning images of different concretes ( Figure 3 and 4 ) can be seen that adding Mingguang attapulgite slurry can increase the cohesion of concrete, while the center of the test block has more cementitious materials and relatively less aggregates, and the distribution of aggregates in the outside is relatively more uniform. When the layer thickness is 6 and 9 cm, the number of large-diameter pores is large and concentrated ( Figure 3 ); The addition of attapulgite-based thixotropic agents and composite admixtures makes the cementitious materials and aggregates in each fault of the concrete evenly distributed and tightly wrapped, and the number of pores in the entire section is significantly reduced and most of them are small pores that are not connected ( Figure 4), which means that the two work together to improve the uniformity of spatial distribution of aggregates and pores in concrete and the characteristics of pore structure. The attapulgite-based thixotropic agent grafted with long-chain organic molecules can efficiently and quickly fill the micro-gaps between cement paste and aggregates, and combine with the free components in the composite admixture to improve the workability, thixotropic properties and water retention of concrete, which is more conducive to forming a stable dense structure and improving the strength of concrete. This is fully reflected in the changes in the CT value and compressive strength of concrete. The CT value and compressive strength of the concrete prepared in Example 2 are 1721.52 Hu and 40.62 Mpa, respectively. After adding the attapulgite-based thixotropic agent and the composite admixture in Example 3, the CT value and compressive strength of the concrete increased to 1905.36 Hu and 46.21 Mpa, respectively, which are much higher than the strength requirements of the crash barrier C30. The other embodiments also show the same trend, showing excellent compactness and toughening and reinforcement properties.
[0015] In summary, the present invention has the following advantages compared with the prior art: 1. The present invention successfully prepares concrete with excellent thixotropy, slump retention, workability and compactness by introducing Mingguang attapulgite thixotropic agent slurry and multifunctional composite admixture into concrete materials, and further combines multiple strategies such as quality control of each component, optimization of mix ratio and step-by-step mixing. It can meet the specific working performance of concrete used in slipform construction, 3D printing and construction of complex structures, and has outstanding advantages in improving construction quality and efficiency, enhancing comprehensive benefits, reducing labor intensity and reducing material consumption. 2. According to the application scenarios of slipform construction and on-site construction requirements, the present invention uses Mingguang attapulgite with thixotropy, large rod crystal length / diameter ratio and high suspension stability as raw material, obtains thixotropic agent slurry through acid activation and surface micro-hydrophobic treatment, and preferably compound multiple components such as collapse preventer, retarder, air entraining agent and high-efficiency water reducer to obtain functional composite admixture, coordinately regulate the macroscopic properties (slump change, strength) and microscopic properties (internal aggregate distribution, pore space distribution) of concrete, and prepare a concrete material with a slump maintained between 130 and 190 mm within 2 hours, high compactness and high strength; 3. The concrete preparation method of the present invention is a method of making minor adjustments based on the conventional concrete mixing process. By adding a small amount of attapulgite-based thixotropic agent and functional admixtures without increasing equipment investment, concrete with specific working performance is obtained, which can be applied to slipform construction or other application fields of thixotropic concrete. Moreover, although the above minor adjustments increase the cost of each cubic meter of concrete by 70 to 100 yuan, they solve many practical technical problems such as transportation, distribution, and paving of slipform construction concrete, with little environmental pollution and ecological damage, and have good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 These are SEM images of Mingguang attapulgite (upper left), Xuyi attapulgite (upper right) and Linze mixed-fiber attapulgite clay (bottom).
[0017] Figure 2 It is the change of slump of prepared concrete over time.
[0018] Figure 3 and 4 They are CT scan images of concrete test blocks prepared in Comparative Example 2 and Example 3, respectively. The size of the concrete test block used is 15 cm x 15 cm. The CT scanning equipment is a Brilliance 16 spiral CT machine, and the specific CT scanning conditions are layer thickness: 3 mm; scanning voltage: 120 kV; reconstruction matrix: 1024×1024; magnification: 1; CT value range: -1024-+3071. After the scanning is completed, the thicknesses of 3, 6, 9, and 12 cm are selected for drawing, and the corresponding aggregate distribution map (above) and pore distribution map (below) are obtained. In the aggregate distribution map, white represents aggregate and gray represents hardened cement paste; in the pore distribution map, black spots represent pores, and the spot size represents the pore diameter size.
[0019] Figure 5 CT values of the concrete test blocks prepared in Comparative Example 2 and Example 3.
[0020] Figure 6 It is the compressive strength of the prepared concrete after 28 days of curing. DETAILED DESCRIPTION
[0021] The method for preparing concrete for sliding film construction by adding attapulgite-based thixotropic agent in the present invention is further described below by means of specific examples. The slump and test block strength are tested in accordance with the standard for testing properties of ordinary concrete mixtures (GB / T50080-2016) and the test procedures for cement and cement concrete for highway engineering (JTG3420-2020).
[0022] Comparative Example 1 Accurately weigh the following raw materials in parts by weight: 315 parts of Portland cement, 55 parts of Class F fly ash, 840 parts of sand (mud content of 1.0%), 310 parts of crushed stone (5-10mm), 720 parts of crushed stone (10-20mm), 168 parts of water, and 5 parts of C6 polycarboxylic acid water reducer. Among them, the sand is natural sand with a mud content of 1.0% and a fineness modulus of 2.8; the mud content of crushed stone is 1.0%; the water reduction rate of the C6 polycarboxylic acid water reducer is 30%. The concrete mixing process is as follows: first, mix the above-mentioned cement, sand, crushed stone, fly ash and other dry materials with water and stir for 2 minutes, then add the water reducer and stir for 3 minutes to obtain concrete. The slump change of this concrete over time and the strength data of the test block after 28 days of curing are shown in Figure 2 and 6 .
[0023] Comparative Example 2 Accurately weigh the following raw materials in parts by weight: 320 parts of silicate cement, 60 parts of F-grade fly ash, 850 parts of sand (mud content of 1.0%), 315 parts of crushed stone (5-10 mm), 720 parts of crushed stone (10-20 mm), 154 parts of water, 5 parts of C6 polycarboxylic acid water reducer, and 28 parts of Mingguang attapulgite slurry. Among them, Mingguang attapulgite slurry is obtained by dispersing Mingguang attapulgite ore (attapulgite content of 75% and MgO mass fraction of 10%) in water with a solid content of 7%, and stirring and hydrating for 12 hours; the sand is natural sand with a mud content of 1.0% and a fineness modulus of 2.8; the mud content in the crushed stone is 1.0%; the water reduction rate of the C6 polycarboxylic acid water reducer is 30%. The concrete mixing process is as follows: first, add water and water reducing agent to the uniformly mixed cement, sand, crushed stone, and fly ash dry materials and stir for 2 minutes, then add Mingguang attapulgite slurry and stir again for 3 minutes to obtain concrete. The slump change of the concrete over time and the strength data of the test block after 28 days of curing are shown in Figure 2 and 6 , the CT scan images and CT values of the concrete specimens are shown in Figure 3 and 5 .
[0024] Example 1 (1) Construction of attapulgite-based thixotropic agent: First, the Mingguang attapulgite ore (attapulgite content of 75% and MgO mass fraction of 10%) was crushed to 100 mesh, ultrasonically dispersed in a phosphoric acid aqueous solution with a pH value of 4.0 and stirred for 8 hours. After filter pressing and centrifugation, the solid phase filter cake was dispersed in an alcohol / water mixed solution containing oleic acid glyceride, wherein the mass of oleic acid glyceride was 0.5% of the mass of acid-activated attapulgite. After reflux stirring at 80°C for 6 hours, centrifugation and drying were performed to obtain a surface slightly hydrophobicized powder. The powder was dispersed in water with a solid content of 5% and stirred for hydration for 24 hours to obtain a thixotropic agent slurry for use. (2) Preparation of composite admixture: accurately weigh the following raw materials in parts by weight: C6 polycarboxylic acid water reducer (water reduction rate: 35%) and sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate in a mass ratio of 100:2:2:2:0.5 and stir (stirring speed: 600 rpm, stirring time: 15 min) to obtain a composite admixture for use; (3) Preparation of concrete mixture: Accurately weigh the following raw materials in parts by weight: 320 parts of silicate cement, 60 parts of Class F fly ash, 850 parts of sand (natural sand, mud content 1.0%, fineness modulus 2.6), 315 parts of crushed stone (5-10mm), 720 parts of crushed stone (10-20mm), 154 parts of water, 5 parts of composite admixture, and 28 parts of attapulgite-based thixotropic agent slurry. The concrete mixing process is as follows: First, add water and composite admixture to the evenly mixed cement, sand, crushed stone, and fly ash dry materials and stir for 2 minutes, then add the attapulgite-based thixotropic agent slurry and stir again for 3 minutes to obtain concrete for sliding film construction. The slump change of this concrete over time and the strength data of the test block after 28 days of curing are shown in Figure 2 and 6 .
[0025] Example 2 (1) Preparation of a attapulgite-based thixotropic agent: First, the Mingguang attapulgite ore (attapulgite content of 75% and MgO mass fraction of 10%) was crushed to 100 mesh, ultrasonically dispersed in a sulfuric acid aqueous solution with a pH value of 3.5 and stirred for 4 hours. After filter pressing and centrifugal separation, the solid phase filter cake was dispersed in an alcohol / water mixed solution containing a silane coupling agent, wherein the mass of the silane coupling agent KH570 was 2.0% of the mass of the acid-activated attapulgite. After reflux stirring at 90°C for 8 hours, the powder was centrifuged and dried to obtain a surface slightly hydrophobicized powder. The powder was dispersed in water with a solid content of 7% and stirred for hydration for 12 hours to obtain a attapulgite-based thixotropic agent slurry for use. (2) Preparation of composite admixture: accurately weigh the following raw materials in parts by weight: C6 polycarboxylic acid water reducer (water reduction rate is 25%) and sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate in a mass ratio of 100:4:2:1:0.25 and stir (stirring speed is 600 rpm, stirring time is 15 min) to obtain a uniform composite admixture for use; (3) Preparation of concrete mixture: accurately weigh the following raw materials in parts by weight: 315 parts of a mixture of silicate cement and sulphoaluminate cement (mass ratio 8:2), 55 parts of Class F fly ash, 840 parts of sand (washed sand, with a mud content and flocculant content of 1.0% and 0.5% respectively, and a fineness modulus of 3.2), 315 parts of crushed stone (5-10 mm), 720 parts of crushed stone (10-20 mm), 154 parts of water, 6 parts of composite admixture, and 26 parts of attapulgite-based thixotropic agent slurry. The concrete mixing process is as follows: first, add water and composite admixture to the uniformly mixed cement, sand, crushed stone, and fly ash dry materials and stir for 2 minutes, then add the attapulgite-based thixotropic agent slurry and stir again for 3 minutes to obtain concrete for sliding film construction. The slump change of the concrete over time and the strength data of the test block after 28 days of curing are shown in 2 and 6.
[0026] Example 3 (1) Preparation of attapulgite-based thixotropic agent: First, the Mingguang attapulgite ore (attapulgite content of 80% and MgO mass fraction of 14%) was crushed to 100 mesh, ultrasonically dispersed in a sulfuric acid aqueous solution with a pH value of 4.0 and stirred for 4 hours. After filter pressing and centrifugation, the solid phase filter cake was dispersed in an alcohol / water mixed solution containing 1.0% oleic acid glyceride, where the mass of oleic acid glyceride was 1.0% of the mass of acid-activated attapulgite. After reflux stirring at 90°C for 8 hours, the powder was centrifuged and dried to obtain a surface slightly hydrophobicized powder. The powder was dispersed in water with a solid content of 7% and stirred for hydration for 24 hours to obtain a attapulgite-based thixotropic agent slurry for use. (2) Preparation of composite admixture: accurately weigh the following raw materials in parts by weight: C6 polycarboxylic acid water reducer (water reduction rate 30%) and sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate in a mass ratio of 100:3:3:1:1.0 and stir (stirring speed 500 rpm, stirring time 20 min) to obtain a uniform composite admixture for use; (3) Preparation of concrete mixture: Accurately weigh the following raw materials in parts by weight: 320 parts of silicate cement, 60 parts of Class F fly ash, 850 parts of sand (natural sand, mud content 0.8%, fineness modulus 2.8), 315 parts of crushed stone (5-10mm), 720 parts of crushed stone (10-20mm), 131 parts of water, 6 parts of composite admixture, and 54 parts of attapulgite-based thixotropic agent slurry. The concrete mixing process is as follows: First, add water and composite admixture to the evenly mixed cement, sand, crushed stone, and fly ash dry materials and stir for 2 minutes, then add the attapulgite-based thixotropic agent slurry and stir again for 3 minutes to obtain concrete for sliding film construction. The slump change of this concrete over time and the strength data of the test block after 28 days of curing are shown in Figure 2 and 6 , CT scan images and CT values are shown in Figure 4 and5 。
Claims
1. A method for preparing concrete for sliding film construction by adding an attapulgite-based thixotropic agent, Features: The concrete is prepared by mixing the following raw materials in parts by weight: 315-320 parts of cement, 55-60 parts of fly ash, 840-850 parts of sand, 305-315 parts of 5-10 mm crushed stone, 720-725 parts of 10-20 mm crushed stone, 180-190 parts of water, 5-6 parts of composite admixture, and 1.5-3.0 parts of attapulgite-based thixotropic agent; wherein the preparation method of the attapulgite-based thixotropic agent is as follows: after pulping acid activation and surface micro-hydrophobic treatment of Mingguang attapulgite ore, it is dispersed in water with a solid content of 5-7%, and stirred and hydrated for at least 12 hours A thixotropic agent slurry is obtained and added in the form of a slurry; the composite admixture is prepared by mixing and compounding a C6 polycarboxylic acid water reducer and sodium gluconate, sodium hexametaphosphate, borax and sodium α-olefin sulfonate (AOS) in a mass ratio of 100:2-4:2-3:1-2:0.25-1.0; the concrete mixing process is as follows: first, 80% of water and the composite admixture are added to the uniformly mixed cement, sand, crushed stone and fly ash dry materials, and stirred for 2-3 minutes, and then the attapulgite-based thixotropic agent slurry is added and stirred again for 2-3 minutes to obtain concrete for sliding film construction.
2. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The cement is any one or more of silicate cement, white cement and sulphoaluminate cement, wherein the dosage of desulfurized gypsum and alcohol amine grinding aids is ≤6% and 0.1% respectively; the fly ash is Class F fly ash, and the water requirement ratio is ≤90%; the mud content in the crushed stone is ≤1.0%.
3. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The attapulgite content in the Mingguang attapulgite ore is ≥75%, and the mass fraction of MgO in the chemical composition tested by XRF is between 10 and 14%.
4. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The sand is natural sand or washed sand, mainly medium-coarse sand, with a fineness modulus of 2.6 to 3.2, wherein the flocculant content in the washed sand is ≤0.5%.
5. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The pulping acid activation is to crush the Mingguang attapulgite ore into 100 meshes, and then ultrasonically disperse it in a sulfuric acid or phosphoric acid aqueous solution with a pH value of 3.5 to 4.0 and stir the reaction for 4 to 8 hours.
6. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The surface micro-hydrophobic treatment process is as follows: first, oleic acid glyceride or silane coupling agent is added to an alcohol-water mixed solution to obtain a uniform modified solution; then, acid-activated attapulgite is ultrasonically dispersed in the above-mentioned modified solution, heated to 80-90° C., refluxed and stirred for 6-8 hours, centrifuged and dried to obtain a surface micro-hydrophobic treated powder, wherein the amount of oleic acid glyceride or silane coupling agent added is 0.5-2.0% of the mass of the acid-activated attapulgite.
7. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 6, Features: In the alcohol-water mixed solution, the volume ratio of alcohol to water is 8:
2.
8. A method for preparing concrete for synovial construction by adding an attapulgite-based thixotropic agent as claimed in claim 1, Features: The slump of the concrete mixture for sliding membrane construction is maintained between 130 and 190 mm within 2 hours.
Citation Information
Patent Citations
Alkali-activated high-performance water reducer and preparation method thereof
CN103011662A
Attapulgite-titanium dioxide modified ultra-high molecular weight polyethylene composite material as well as preparation method and application thereof
CN112226264A
Method for regulating and controlling performance of cement mortar by adding attapulgite-based modified material
CN117550852A
Highway bridge high pier slip form concrete and preparation method thereof
CN118221399A