A kind of high thixotropic conductive silver paste and preparation method thereof
By combining modified silver powder and glass powder, a highly thixotropic conductive silver paste was prepared, which solved the problem of insufficient fluidity and thixotropy of the conductive silver paste, and improved the printing performance and the efficiency of the solar cell.
Patent Information
- Application Number
- CN202410885192.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The existing conductive silver paste lacks fluidity and thixotropy during the printing process, resulting in unclear boundaries of the printing ink film and low resolution, which affects the photoelectric conversion efficiency and power generation cost of crystalline silicon solar cells.
By uniformly mixing the glass powder and the modified silver powder, adding organic solvent, thickener and thixotropic agent, a highly thixotropic conductive silver paste is prepared, and the sintering of the silver paste is reduced by using the spherical structure of the modified silver powder and the bismuth element coating technology. Temperature and specific contact resistance, and improve the wetting performance of metal on the ceramic surface through glass powder.
The prepared conductive silver paste has good fluidity and thixotropy, and can be transferred to the printing material smoothly, ensuring clear boundaries and high resolution of the printing ink film, reducing the sintering temperature and specific contact resistance of the silver paste, and improving the solar cell photoelectric conversion efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery materials, and in particular to a highly thixotropic conductive silver paste and a preparation method thereof. Background Art
[0002] Solar energy can provide huge energy for social and economic development. Crystalline silicon solar cells are the most widely used photovoltaic cells with the most mature preparation technology. Conductive paste, as an important raw material for crystalline silicon solar cells, has a great impact on the photoelectric conversion efficiency and power generation cost of the cells. Conductive paste for crystalline silicon solar cells is divided into front silver paste, back silver paste and back aluminum paste according to its use and printing location.
[0003] Silver paste is divided into front silver paste and back silver paste according to the different printing parts; back silver paste is the material that constitutes the negative electrode of the battery. Since the back silver and back aluminum paste are printed on the same side of the battery, the matching of the back silver paste and the back aluminum paste needs to be considered during preparation to reduce the cracks between the silver and aluminum electrodes. The efficiency of the positive electrode composed of the front silver paste in absorbing current determines the photoelectric conversion efficiency of the solar cell. Therefore, the front silver paste needs to have a good ohmic contact with the silicon substrate. The smaller the contact resistance of the front silver paste, the better the conductivity and the higher the battery efficiency. Since the width of the front silver fine grid line is only about 0.1mm, the front silver paste needs to have a suitable aspect ratio when printing. However, since the conductive silver paste contains a large amount of metallic silver particles, it has a different printing suitability from ordinary ink. The volume fraction of silver particles in the conductive silver paste is different, and its fluidity and thixotropy are also different. Good fluidity enables the silver paste to be smoothly transferred from printing to the substrate, and good thixotropy is the guarantee for achieving clear boundaries and high resolution of the conductor printing ink film. Summary of the invention
[0004] The purpose of the present invention is to provide a highly thixotropic conductive silver paste and a preparation method thereof. The prepared conductive silver paste has good fluidity, so that the silver paste can be smoothly transferred from printing to a printing material, and the obtained conductor printing ink film has clear boundaries and high resolution.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A method for preparing a highly thixotropic conductive silver paste comprises the following steps:
[0007] S1: mixing glass powder and modified silver powder uniformly to obtain a solid mixture;
[0008] S2: adding an organic solvent into a reaction kettle, controlling the temperature at 45-55°C, adding a thickener, keeping the temperature for 1-3 hours under stirring, adding a thixotropic agent, and keeping the temperature for 0.5-1 hour under stirring to obtain an organic carrier;
[0009] S3: pouring the slurry obtained by mixing the organic carrier and the solid mixture into a three-roll grinder and grinding it to obtain a conductive silver paste;
[0010] The preparation method of modified silver powder comprises the following steps:
[0011] A1: Add thioglycolic acid into a reaction kettle, add sodium hydroxide solution to adjust the pH to 7, add silver powder, stir at room temperature for 15-30 minutes, filter, wash with water, and dry to obtain organic silver powder;
[0012] A2: Add bismuth nitrate and methanol into a reaction kettle and disperse them evenly, add organic silver powder and disperse them evenly, let it stand at room temperature for 12-24 hours, filter, take the remaining solid and place it in a reducing atmosphere, at 200-210°C, react for 12-18 hours to obtain modified silver powder.
[0013] As a further solution of the present invention: the sodium hydroxide aqueous solution in A1 is 3-5 mol / L sodium hydroxide aqueous solution; the mass ratio of thioglycolic acid:silver powder is 0.1-0.3:1.
[0014] As a further solution of the present invention: the addition ratio of bismuth nitrate, methanol and organic silver powder in A2 is 0.1-0.2g:50-100mL:1g.
[0015] As a further embodiment of the present invention: the reducing atmosphere in A2 contains 5-7% hydrogen and the rest is nitrogen.
[0016] As a further solution of the present invention: the conductive silver paste includes the following raw materials in weight percentage: 1-3% glass powder, 85-95% modified silver powder, and 8-10% organic carrier; the sum of the weight percentages of the raw materials is 100%.
[0017] As a further solution of the present invention: the silver powder includes 20-25wt% of spherical aluminum powder with a particle size of 1-3um and 75-80wt% of spherical aluminum powder with a particle size of 5-8um.
[0018] As a further solution of the present invention: the organic solvent is obtained by mixing propylene glycol methyl ether acetate and dibutyl phthalate, wherein the propylene glycol methyl ether acetate accounts for 40-55% of the total mass of the organic carrier; and the dibutyl phthalate accounts for 30-35% of the total mass of the organic carrier.
[0019] As a further solution of the present invention: the thickener is any one of ethyl cellulose, nitrocellulose, cellulose butyrate, butyl cellulose and hydroxy cellulose, and the thickener accounts for 4-6% of the total mass of the organic carrier.
[0020] As a further solution of the present invention: the thixotropic agent is obtained by mixing hydrogenated castor oil and polyamide wax in a mass ratio of 1:1-1.1, and the thixotropic agent accounts for 3-6% of the total mass of the organic carrier.
[0021] A highly thixotropic conductive silver paste is prepared by any one of the above preparation methods.
[0022] Beneficial effects of the present invention:
[0023] The present invention uses the mercapto group of thioglycolic acid to react with silver powder, grafts carboxyl groups on the surface of the silver powder, and obtains an organic silver powder; and utilizes the carboxyl groups on the surface of the organic silver powder to deprotonate and chelate and bridge with bismuth ions, and then undergoes a reduction reaction, and coats the surface of the silver powder with bismuth elements to obtain modified silver powder. The present invention performs an organic treatment on the silver powder to enhance the wettability of the particle surface to the dispersion medium, so that the conductive particles spontaneously repel each other to form a dispersed slurry with good stability; and with the addition of bismuth elements, the sintering temperature of the silver paste is effectively reduced, and the square resistance and specific contact resistance of the silver paste are reduced.
[0024] The modified silver powder of the present application adopts spherical silver powder as a base material. The spherical silver powder has a high sphericity. The prepared silver paste has good fluidity and can pass through the positive electrode fine grid line well. Large-diameter and small-diameter silver particles are filled with each other to ensure sufficient contact area, so that the silver paste has good density. The present application uses glass powder as an inorganic adhesive to improve the wetting performance of metal on the ceramic surface. The glass powder can bond the silver powder after melting. The glass powder system can melt and etch the anti-reflection layer on the upper part of the silicon substrate, so that the silver powder forms an ohmic contact with the silicon substrate. At the same time, it can also be used as a sintering aid to reduce the sintering temperature.
[0025] In the organic carrier of the present application, propylene glycol methyl ether acetate and dibutyl phthalate are used as organic solvents; wherein, propylene glycol methyl ether acetate is used as a low-boiling solvent and dibutyl phthalate is used as a high-boiling solvent, which can plasticize the thickener in the organic carrier, and dibutyl phthalate is inserted between the ethyl cellulose molecular chains to weaken the intermolecular forces, increase the distance and activity space between the ethyl cellulose molecular chains, increase the plasticity of the slurry, and effectively improve the viscosity of the carrier system; and thickeners and thixotropic agents are added to the organic carrier, and the thickener can increase the viscosity of the slurry, so that the silver powder particles in the slurry remain in a suspended emulsified state, prevent precipitation, and make the slurry convenient for screen printing; the organic carrier prepared by the present application makes the inorganic binding phase and the conductive particles in the slurry fully wetted, giving the conductive slurry excellent viscosity, volatility and thixotropy. The silver paste prepared by the present application has excellent thixotropy, can be stably volatilized between 120-400°C, and meets the needs of solar cells. DETAILED DESCRIPTION
[0026] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] The preparation method of modified silver powder comprises the following steps:
[0029] A1: Add 0.1g of thioglycolic acid into a reaction kettle, add 5mol / L sodium hydroxide aqueous solution to adjust the pH to 7, add 1g of silver powder (0.25g of spherical aluminum powder with a particle size of 1-3um, 0.75g of spherical aluminum powder with a particle size of 5-8um), stir at room temperature for 15min, filter, wash with water, and dry to obtain organic silver powder;
[0030] A2: Add 0.1g bismuth nitrate and 50mL methanol into a reactor and disperse them evenly, add 1g organic silver powder and disperse them evenly, let it stand at room temperature for 12h, filter, take the remaining solid and place it in a reducing atmosphere, react at 200℃ for 12h, the reducing atmosphere contains 7% hydrogen and the rest is nitrogen; obtain modified silver powder.
[0031] Example 2
[0032] The preparation method of modified silver powder comprises the following steps:
[0033] A1: Add 0.2g of thioglycolic acid into a reaction kettle, add 5mol / L sodium hydroxide aqueous solution to adjust the pH to 7, add 1g of silver powder (0.25g of spherical aluminum powder with a particle size of 1-3um, 0.75g of spherical aluminum powder with a particle size of 5-8um), stir at room temperature for 20min, filter, wash with water, and dry to obtain organic silver powder;
[0034] A2: Add 0.15g bismuth nitrate and 70mL methanol into a reactor and disperse them evenly, add 1g organic silver powder and disperse them evenly, let it stand at room temperature for 18h, filter, take the remaining solid and place it in a reducing atmosphere, react at 200℃ for 15h, the reducing atmosphere contains 7% hydrogen and the rest is nitrogen; obtain modified silver powder.
[0035] Example 3
[0036] The preparation method of modified silver powder comprises the following steps:
[0037] A1: Add 0.3g of thioglycolic acid into a reaction kettle, add 5mol / L sodium hydroxide aqueous solution to adjust the pH to 7, add 1g of silver powder (0.25g of spherical aluminum powder with a particle size of 1-3um, 0.75g of spherical aluminum powder with a particle size of 5-8um), stir at room temperature for 30min, filter, wash with water, and dry to obtain organic silver powder;
[0038] A2: Add 0.2g bismuth nitrate and 100mL methanol into a reactor and disperse them evenly, add 1g organic silver powder and disperse them evenly, let it stand at room temperature for 24h, filter, take the remaining solid and place it in a reducing atmosphere at 210℃, react for 18h, the reducing atmosphere contains 7% hydrogen and the rest is nitrogen; obtain modified silver powder.
[0039] Example 4
[0040] A method for preparing a highly thixotropic conductive silver paste comprises the following steps:
[0041] S1: According to the following glass powder composition, pour the glass powder raw material into a platinum crucible, place it in a muffle furnace at 1300°C for 10 minutes, pour the glass melt into deionized water for quenching and ball milling to obtain glass powder; the glass powder includes the following raw materials in weight percentage: 0.12% K2O, 0.12% WO3, 0.11% TeO, 0.27% ZnO, 1.55% Zn3(PO4)2·4H2O, 2.01% Bi2O, 2.04% SiO2, 2.36% Na2O, 2.61% Al2O3, 3.67% Li2O, 4.7% Mg, 8.14% TiO2, 9.23% B2O3, 12% CaO, 50.1% PbO;
[0042] S2: 1.3 g of glass powder and 90 g of the modified silver powder prepared in Example 1 were mixed uniformly to obtain a solid mixture;
[0043] S3: 55 g of propylene glycol methyl ether acetate and 35 g of dibutyl phthalate were added to a reaction kettle and dispersed evenly, the temperature was controlled at 45°C, 6% of ethyl fiber was added, and the mixture was kept warm for 1 h under stirring, 2 g of hydrogenated castor oil and 2 g of polyamide wax were added, and the mixture was kept warm for 0.5 h under stirring to obtain an organic carrier;
[0044] S4: Pour the slurry obtained by mixing 8.7 g of the organic vehicle and 91.3 g of the solid mixture into a three-roll mill and grind to obtain a conductive silver paste.
[0045] Example 5
[0046] A method for preparing a highly thixotropic conductive silver paste comprises the following steps:
[0047] S1: According to the following glass powder composition, pour the glass powder raw material into a platinum crucible, place it in a muffle furnace at 1300°C for 10 minutes, pour the glass melt into deionized water for quenching and ball milling to obtain glass powder; the glass powder includes the following raw materials in weight percentage: 0.12% K2O, 0.12% WO3, 0.11% TeO, 0.27% ZnO, 1.55% Zn3(PO4)2·4H2O, 2.01% Bi2O, 2.04% SiO2, 2.36% Na2O, 2.61% Al2O3, 3.67% Li2O, 4.7% Mg, 8.14% TiO2, 9.23% B2O3, 12% CaO, 50.1% PbO;
[0048] S2: 1.3 g of glass powder and 90 g of modified silver powder prepared in Example 2 were mixed uniformly to obtain a solid mixture;
[0049] S3: 55 g of propylene glycol methyl ether acetate and 35 g of dibutyl phthalate were added to a reaction kettle and dispersed evenly, the temperature was controlled at 45°C, 6% of ethyl fiber was added, and the mixture was kept warm for 1 h under stirring, 2 g of hydrogenated castor oil and 2 g of polyamide wax were added, and the mixture was kept warm for 0.5 h under stirring to obtain an organic carrier;
[0050] S4: Pour the slurry obtained by mixing 8.7 g of the organic vehicle and 91.3 g of the solid mixture into a three-roll mill and grind to obtain a conductive silver paste.
[0051] Example 6
[0052] A method for preparing a highly thixotropic conductive silver paste comprises the following steps:
[0053] S1: According to the following glass powder composition, pour the glass powder raw material into a platinum crucible, place it in a muffle furnace at 1300°C for 10 minutes, pour the glass melt into deionized water for quenching and ball milling to obtain glass powder; the glass powder includes the following raw materials in weight percentage: 0.12% K2O, 0.12% WO3, 0.11% TeO, 0.27% ZnO, 1.55% Zn3(PO4)2·4H2O, 2.01% Bi2O, 2.04% SiO2, 2.36% Na2O, 2.61% Al2O3, 3.67% Li2O, 4.7% Mg, 8.14% TiO2, 9.23% B2O3, 12% CaO, 50.1% PbO;
[0054] S2: 1.3 g of glass powder and 90 g of the modified silver powder prepared in Example 3 were mixed uniformly to obtain a solid mixture;
[0055] S3: 55 g of propylene glycol methyl ether acetate and 35 g of dibutyl phthalate were added to a reaction kettle and dispersed evenly, the temperature was controlled at 45°C, 6% of ethyl fiber was added, and the mixture was kept warm for 1 h under stirring, 2 g of hydrogenated castor oil and 2 g of polyamide wax were added, and the mixture was kept warm for 0.5 h under stirring to obtain an organic carrier;
[0056] S4: Pour the slurry obtained by mixing 8.7 g of the organic vehicle and 91.3 g of the solid mixture into a three-roll mill and grind to obtain a conductive silver paste.
[0057] Comparative Example 1
[0058] The preparation method of modified silver powder comprises the following steps:
[0059] 0.1 g of thioglycolic acid was added to the reaction kettle, 5 mol / L sodium hydroxide aqueous solution was added to adjust the pH to 7, 1 g of silver powder (0.25 g of spherical aluminum powder with a particle size of 1-3 um, 0.75 g of spherical aluminum powder with a particle size of 5-8 um) was added, stirred at room temperature for 15 min, filtered, washed with water, and dried to obtain modified silver powder.
[0060] Comparative Example 2
[0061] The preparation method of modified silver powder comprises the following steps:
[0062] Disperse 0.1 g of bismuth nitrate and 1 g of silver powder evenly, let stand at room temperature for 12 hours, filter, take the remaining solid and place it in a reducing atmosphere, react at 200°C for 12 hours, the reducing atmosphere contains 7% hydrogen and the rest is nitrogen; obtain modified silver powder.
[0063] Comparative Example 3
[0064] Compared with Example 4, Comparative Example 3 only replaces the modified silver powder prepared in Example 1 added in Example 4 with an equal amount of the modified silver powder prepared in Comparative Example 1, and the remaining components and preparation method are completely consistent with Example 4.
[0065] Comparative Example 4
[0066] Compared with Example 4, Comparative Example 3 only replaces the modified silver powder prepared in Example 1 added in Example 4 with the modified silver powder prepared in Comparative Example 2 in equal amount, and the remaining components and preparation method are completely consistent with Example 4.
[0067] Performance Testing
[0068] (1) Thixotropy: The viscosity was measured using a Brookfield rotary viscometer (rotor No. 14) at rotor speeds of 5 r / min and 50 r / min, and the thixotropic index It was calculated according to the following formula:
[0069] It=η5 / η50
[0070] Where, It is the thixotropic index; η5 is the viscosity measured when the rotor speed is 5 r / min; η50 is the viscosity measured when the rotor speed is 50 r / min; the test results are shown in Table 2;
[0071] (2) Fineness: Stir the roller-milled slurry thoroughly with an oiling knife. Pour a small amount of slurry into the deep part of the groove of the scraper fineness gauge to fill the groove. Make the scraper perpendicular to the surface of the scraper fineness gauge and pull the scraper from the deep part of the groove to the shallow part at a suitable speed to fill the groove with slurry. Observe the slurry in the groove. When the slurry begins to have rough and uneven particles, that is the reading position. The test results are shown in Table 2.
[0072] (3) Specific resistance:
[0073] a: The front silver paste prepared in Examples 4-6 and Comparative Examples 3-4 was printed on a silicon wafer using a high-resolution screen printer. The silicon wafer used was a 5-inch 1 / 4 single crystal silicon wafer (the silicon wafer had been cleaned, textured, diffused and anti-reflection coated before printing the silver paste); the printing screen was a stainless steel screen with 300 mesh, 30N tension, 45° orientation angle, and a grid line width of 80μm;
[0074] b: The cell with printed positive silver electrode is sintered in a 9-zone infrared chain tunnel furnace. Sintering process: The temperature settings of each zone are shown in Table 1. The conveyor belt speed of the sintering furnace is 5.8 m / min. -1 ;
[0075] Table 1: Battery sintering temperature zone parameters
[0076] Temperature Zone 1 2 3 4 5 6 7 8 9 Temperature / ℃ 320 340 350 520 570 610 650 720 750
[0077] c: The resistance test was performed using a Napson Cresbox RT-80 four-point probe resistance meter, and the contact resistance test was performed using the transmission line method; the test results are shown in Table 2;
[0078] Table 2: Statistical table of silver paste performance test data for Examples 4-6 and Comparative Examples 3-4
[0079]
[0080] As can be seen from Table 2, the modified silver powder prepared in the present application is added to the silver paste, and the prepared silver paste can pass through the positive silver ultra-fine grid lines and has good printing performance; and the thixotropic index is high, so that the grid lines printed by the paste have a larger aspect ratio.
[0081] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for preparing a highly thixotropic conductive silver paste, characterized in that: The steps include: S1: mixing glass powder and modified silver powder uniformly to obtain a solid mixture; S2: adding an organic solvent into a reaction kettle, controlling the temperature at 45-55°C, adding a thickener, keeping the temperature for 1-3 hours under stirring, adding a thixotropic agent, and keeping the temperature for 0.5-1 hour under stirring to obtain an organic carrier; S3: pouring the slurry obtained by mixing the organic carrier and the solid mixture into a three-roll grinder and grinding it to obtain a conductive silver paste; The preparation method of the modified silver powder comprises the following steps: A1: Add thioglycolic acid into a reaction kettle, add sodium hydroxide solution to adjust the pH to 7, add silver powder, stir at room temperature for 15-30 minutes, filter, wash with water, and dry to obtain organic silver powder; A2: Add bismuth nitrate and methanol into a reaction kettle and disperse them evenly, add organic silver powder and disperse them evenly, let it stand at room temperature for 12-24 hours, filter, take the remaining solid and place it in a reducing atmosphere, at 200-210°C, react for 12-18 hours to obtain modified silver powder; The organic solvent is obtained by mixing propylene glycol methyl ether acetate and dibutyl phthalate, wherein the propylene glycol methyl ether acetate accounts for 40-55% of the total mass of the organic carrier; and the dibutyl phthalate accounts for 30-35% of the total mass of the organic carrier.
2. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The sodium hydroxide aqueous solution in A1 is 3-5 mol / L sodium hydroxide aqueous solution; the mass ratio of thioglycolic acid:silver powder is 0.1-0.3:
1.
3. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The addition ratio of bismuth nitrate, methanol and organic silver powder in A2 is 0.1-0.2g:50-100mL:1g.
4. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The reducing atmosphere in A2 contains 5-7% hydrogen and the rest is nitrogen.
5. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The conductive silver paste comprises the following raw materials in weight percentage: 1-3% glass powder, 85-95% modified silver powder, and 8-10% organic carrier; the sum of the weight percentages of the raw materials is 100%.
6. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The silver powder comprises 20-25wt% of spherical aluminum powder with a particle size of 1-3um and 75-80wt% of spherical aluminum powder with a particle size of 5-8um.
7. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The thickener is any one of ethyl cellulose, nitrocellulose, cellulose butyrate, butyl cellulose and hydroxy cellulose, and the thickener accounts for 4-6% of the total mass of the organic carrier.
8. The method for preparing a highly thixotropic conductive silver paste according to claim 1, characterized in that: The thixotropic agent is obtained by mixing hydrogenated castor oil and polyamide wax in a mass ratio of 1:1-1.1, and the thixotropic agent accounts for 3-6% of the total mass of the organic carrier.
9. A highly thixotropic conductive silver paste, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Electric conductive silver paste and manufacturing method thereof
CN103258584A
Silicon solar cell front silver electrode high-square-resistance slurry and manufacturing method thereof
CN103440897A
Silicon solar cell front face electrode silver paste and preparing method thereof
CN104157328A
UV conductive silver paste formula and preparation method thereof
CN107403657A
Front electrode silver paste for solar battery, silver powder and preparation method thereof