Molybdenum-copper composite material sintered part and preparation method thereof
Through microwave sintering technology and specific ingredients combination of molybdenum-copper composites, the long-term problem of high temperature in the existing sintering method is solved, and the sintering of high-efficiency and energy-saving molybdenum-copper composites is achieved, which improves the strength and density of the material and improves heat conduction Conductive properties.
Patent Information
- Application Number
- CN202411028640.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing molybdenum-copper composite sintering methods have long sintering time and high temperature, resulting in waste of energy, low density, and poor thermal conductivity.
Using microwave sintering technology, the molybdenum powder, copper powder and ingredients (containing tungsten powder and activated elements such as nickel powder or chromium powder) are configured according to a specific mass ratio, mix evenly and press it into a green body, and use microwave heating to quickly sinter it at low temperature. The sintering temperature decreases, the time is shortened, and the atmosphere is nitrogen.
The high strength and ablation resistance of molybdenum-copper composite materials are achieved, the sintering temperature is greatly reduced, the time is shortened, the material density is improved, the energy-saving effect is significant, the internal thermal stress is reduced, and the diffusion coefficient is improved.
Smart Images

Figure CN118957386A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a molybdenum-copper composite material sintered component and a preparation method thereof. Background Art
[0002] Molybdenum-copper composite material is a uniform mixture of two-phase monomers composed of molybdenum and copper, which are neither mutually soluble nor form intermetallic compounds. It is generally called molybdenum-copper pseudoalloy. It is this combination that makes the molybdenum-copper composite material have the characteristics of high temperature resistance, high strength and high density of molybdenum, and high electrical conductivity, high thermal conductivity and high plasticity of copper, making it widely used in various fields such as aerospace, electronics, machinery, metallurgy, and electrical appliances.
[0003] After searching, the patent with the authorization publication number CN114000023B discloses a method for preparing molybdenum-copper composite materials by gas pressure infiltration sintering, which specifically includes the following steps: step 1, selecting the particle size of molybdenum powder, copper powder and nickel powder; step 2, weighing molybdenum powder with the particle size selected in step 1 to prepare mixed powder. The problem of low density and poor thermal and electrical conductivity of molybdenum-copper composite materials prepared by the existing method is solved, but the above patent has a long sintering time and high temperature, which wastes energy. Therefore, a molybdenum-copper composite material sintered component and its preparation method are proposed. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a molybdenum-copper composite material sintered component and a preparation method thereof, which achieves the purpose of significantly reducing the sintering temperature, shortening the sintering time, and being more energy-efficient by changing the sintering method.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A molybdenum-copper composite material sintered component comprises the following components by mass ratio: molybdenum powder, copper powder and ingredients, wherein the molybdenum powder accounts for 5-45wt%, the copper powder accounts for 8-40wt% and the ingredients account for 20-55wt%.
[0009] Furthermore, the ingredients include tungsten powder and activation elements, wherein the tungsten powder accounts for 12-30wt% and the activation elements account for 8-25wt%, and the activation elements are nickel powder or chromium powder.
[0010] On the basis of the above scheme, the ingredients are tungsten powder and ethanol, the tungsten powder accounts for 12-30wt% and the ethanol accounts for 8-25wt%.
[0011] The present invention also provides a method for preparing a molybdenum-copper composite material sintered component, comprising the following steps:
[0012] S1: Prepare raw materials according to the mass ratio;
[0013] S2: Mixing, mixing the raw materials evenly;
[0014] S3: Pressing into green compacts, pressing the mixed powder into green compacts with a relative density of 68%-78% in a mold;
[0015] S4: high temperature sintering, placing the green body in a heating device, heating the green body with microwaves, heating the green body to 200°C and keeping it warm for 7-21 minutes, then heating it to 850-1300°C at a heating rate of 15-45°C / min and keeping it warm for 25-45 minutes, then turning off the power and cooling it with the furnace to obtain the sintered molybdenum-copper composite material.
[0016] Furthermore, the raw materials in S1 include copper powder with a particle size of 30-60μm, molybdenum powder, tungsten powder and nickel powder with a particle size of 1-3μm, the tungsten powder is composed of fine-grained tungsten powder and medium-grained tungsten powder in a mass ratio of (1-3): (1-3), or the tungsten powder is composed of fine-grained tungsten powder, medium-grained tungsten powder and coarse-grained tungsten powder in a mass ratio of (1-3): (1-3): (1-3); the average particle size of the fine-grained tungsten powder is 1-6μm, the average particle size of the medium-grained tungsten powder is 10-30μm, the average particle size of the coarse-grained tungsten powder is 70-100μm, and the average particle size of the nickel powder is 2-9μm.
[0017] On the basis of the above scheme, the sintering atmosphere in S4 is nitrogen.
[0018] (III) Beneficial effects
[0019] Compared with the prior art, the present invention provides a molybdenum-copper composite material sintered component and a preparation method thereof, which has the following beneficial effects:
[0020] 1. In the present invention, molybdenum can solid-solution strengthen the tungsten matrix and play a role in solid-solution strengthening. The activated elements can increase the density of the material, so that the prepared molybdenum-copper composite material has higher strength and ablation resistance and other properties.
[0021] 2. The microwave sintering adopted in the present invention relies on the material itself to absorb microwave energy and convert it into kinetic energy and potential energy of the molecules inside the material. The material is heated evenly inside and outside at the same time, so that the internal thermal stress of the material can be reduced to a minimum, and the sintering temperature is greatly reduced, the sintering time is shortened, and it is more energy-saving.
[0022] 3. Under the action of microwave electromagnetic energy, the kinetic energy of molecules or ions inside the material of the present invention increases, so that the sintering activation energy is reduced and the diffusion coefficient is increased, so that low-temperature rapid sintering can be performed. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1This is a schematic diagram of the process structure of a method for preparing a molybdenum-copper composite material sintered component proposed in the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] Reference Figure 1 A molybdenum-copper composite material sintered component, the materials of which include the following components by mass ratio: molybdenum powder, copper powder, and ingredients, wherein molybdenum powder accounts for 25wt%, copper powder accounts for 35wt%, and ingredients account for 40wt%. The ingredients include tungsten powder and activation elements, tungsten powder accounts for 21wt%, and the activation element is nickel powder accounting for 19wt%.
[0027] The present invention also proposes a method for preparing a molybdenum-copper composite material sintered component, comprising the following steps:
[0028] S1: preparing raw materials, and preparing the raw materials according to the mass ratio. The raw materials in S1 include copper powder with a particle size of 40 μm, molybdenum powder, tungsten powder and nickel powder with a particle size of 1-3 μm. The tungsten powder is composed of fine-grained tungsten powder and medium-grained tungsten powder in a mass ratio of (2): (2), or the tungsten powder is composed of fine-grained tungsten powder, medium-grained tungsten powder and coarse-grained tungsten powder in a mass ratio of (1): (2): (1); the average particle size of the fine-grained tungsten powder is 5 μm, the average particle size of the medium-grained tungsten powder is 15 μm, the average particle size of the coarse-grained tungsten powder is 80 μm, and the average particle size of the nickel powder is 5 μm. Molybdenum can solid solution strengthen the tungsten matrix and play a role in solid solution strengthening. The activation element can improve the density of the material, so that the prepared molybdenum-copper composite material has high strength and ablation resistance and other properties;
[0029] S2: Mixing, mixing the raw materials evenly;
[0030] S3: Pressing into green compacts, pressing the mixed powder into green compacts with a relative density of 75% in a mold;
[0031] S4: high temperature sintering, placing the green body in a heating device, heating the green body with microwaves, heating the green body to 200°C and keeping it warm for 10 minutes, then continuing to heat it to 850°C at a heating rate of 20°C / min and keeping it warm for 30 minutes, then turning off the power and cooling it with the furnace to obtain the sintered molybdenum-copper composite material. The microwave sintering adopted relies on the material itself to absorb microwave energy and convert it into the kinetic energy and potential energy of the molecules inside the material. The material is heated evenly inside and outside at the same time, so that the internal thermal stress of the material can be reduced to a minimum, and the sintering temperature is greatly reduced, the sintering time is shortened, and it is more energy-efficient. Secondly, under the action of microwave electromagnetic energy, the kinetic energy of the molecules or ions inside the material increases, which reduces the sintering activation energy and increases the diffusion coefficient, so that low-temperature rapid sintering can be performed. The sintering atmosphere in S4 is nitrogen.
[0032] Example 2
[0033] Reference Figure 1 A molybdenum-copper composite material sintered component, whose materials include the following components in mass ratio: molybdenum powder, copper powder, and ingredients, wherein molybdenum powder accounts for 25wt%, copper powder accounts for 35wt%, and ingredients account for 40wt%. The ingredients include tungsten powder and activation elements, tungsten powder accounts for 20wt%, the activation element is chromium powder accounting for 20wt%, and the activation element is or chromium powder.
[0034] The present invention also proposes a method for preparing a molybdenum-copper composite material sintered component, comprising the following steps:
[0035] S1: preparing raw materials, preparing raw materials according to mass ratio, wherein the raw materials in S1 include copper powder with a particle size of 45 μm, molybdenum powder, tungsten powder and chromium powder with a particle size of 2 μm, the tungsten powder is composed of fine-grained tungsten powder and medium-grained tungsten powder in a mass ratio of (2):(2), or the tungsten powder is composed of fine-grained tungsten powder, medium-grained tungsten powder and coarse-grained tungsten powder in a mass ratio of (2):(1):(1); the average particle size of the fine-grained tungsten powder is 3 μm, the average particle size of the medium-grained tungsten powder is 20 μm, the average particle size of the coarse-grained tungsten powder is 85 μm, and the average particle size of the chromium powder is 6 μm. Molybdenum can solid solution strengthen the tungsten matrix and play a role in solid solution strengthening. The activation element can improve the density of the material, so that the prepared molybdenum-copper composite material has high strength and ablation resistance and other properties;
[0036] S2: Mixing, mixing the raw materials evenly;
[0037] S3: Pressing into green compacts, pressing the mixed powder into green compacts with a relative density of 72% in a mold;
[0038] S4: high temperature sintering, placing the green body in a heating device, heating the green body with microwaves, heating the green body to 200°C and keeping it warm for 12 minutes, then continuing to heat it to 1000°C at a heating rate of 28°C / min and keeping it warm for 32 minutes, then turning off the power and cooling it with the furnace to obtain the sintered molybdenum-copper composite material. The microwave sintering adopted relies on the material itself to absorb microwave energy and convert it into the kinetic energy and potential energy of the molecules inside the material. The material is heated evenly inside and outside at the same time, so that the internal thermal stress of the material can be reduced to a minimum, and the sintering temperature is greatly reduced, the sintering time is shortened, and it is more energy-efficient. Secondly, under the action of microwave electromagnetic energy, the kinetic energy of the molecules or ions inside the material increases, which reduces the sintering activation energy and increases the diffusion coefficient, so that low-temperature rapid sintering can be performed. The sintering atmosphere in S4 is nitrogen.
[0039] In the description of this article, it should be noted that relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
Claims
1. A molybdenum-copper composite material sintered component, characterized in that: The material comprises the following components by weight: molybdenum powder, copper powder and ingredients, wherein the molybdenum powder accounts for 5-45wt%, the copper powder accounts for 8-40wt% and the ingredients account for 20-55wt%.
2. A molybdenum-copper composite material sintered component according to claim 1, characterized in that: The ingredients include tungsten powder and activation elements, wherein the tungsten powder accounts for 12-30wt% and the activation elements accounts for 8-25wt%, and the activation elements are nickel powder or chromium powder.
3. A molybdenum-copper composite material sintered component according to claim 1, characterized in that: The ingredients are tungsten powder and ethanol, wherein the tungsten powder accounts for 12-30wt% and the ethanol accounts for 8-25wt%.
4. A method for preparing a sintered molybdenum-copper composite material component, characterized in that: The following steps are involved: S1: Prepare raw materials according to the mass ratio; S2: Mixing, mixing the raw materials evenly; S3: Pressing into green compacts, pressing the mixed powder into green compacts with a relative density of 68%-78% in a mold; S4: high temperature sintering, placing the green body in a heating device, heating the green body with microwaves, heating the green body to 200°C and keeping it warm for 7-21 minutes, then heating it to 850-1300°C at a heating rate of 15-45°C / min and keeping it warm for 25-45 minutes, then turning off the power and cooling it with the furnace to obtain the sintered molybdenum-copper composite material.
5. The method for preparing a sintered molybdenum-copper composite material component according to claim 4, characterized in that: The raw materials in S1 include copper powder with a particle size of 30-60μm, molybdenum powder, tungsten powder and nickel powder with a particle size of 1-3μm, the tungsten powder is composed of fine-grained tungsten powder and medium-grained tungsten powder in a mass ratio of (1-3):(1-3), or the tungsten powder is composed of fine-grained tungsten powder, medium-grained tungsten powder and coarse-grained tungsten powder in a mass ratio of (1-3):(1-3):(1-3); the average particle size of the fine-grained tungsten powder is 1-6μm, the average particle size of the medium-grained tungsten powder is 10-30μm, the average particle size of the coarse-grained tungsten powder is 70-100μm, and the average particle size of the nickel powder is 2-9μm.
6. The method for preparing a sintered molybdenum-copper composite material component according to claim 1, characterized in that: The sintering atmosphere in S4 is nitrogen.
Citation Information
Cited By
Rapid preparation method of fine-grain high-strength molybdenum-based alloy
CN120400594A
A rapid preparation method of fine-grain high-strength molybdenum-based alloy
CN120400594B