Preparation method of road edge stone
The treatment of waste materials by high-performance cement, polymer emulsion and chemical stabilizers improves the durability and environmental protection of curbs, solves the problems of unstable strength and pollution of waste preparation curbs, and realizes environmentally friendly and efficient curbs preparation.
Patent Information
- Application Number
- CN202411286558.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing curb stone preparation technology, the use of industrial waste and construction waste causes unstable and low curb stone strength, and the waste tire powder contains volatile organic compounds and heavy metals, which affects environmental quality and durability.
Use high-performance ordinary silicate cement or cement mixed with nanomaterials, waste construction aggregate, waste tire glue powder, silica fume, fly ash, polymer emulsion and water to treat waste tires through silane and silicone Glue powder, polymer emulsion modify waste aggregate, control the water-gluing ratio, form a stable chemical bonding and protective film, and improve the strength and durability of concrete.
The durability of curbs prepared from waste is close to standard aggregate, reducing pollution risks and negative environmental impacts, and ensuring the performance stability and environmental protection of finished curbs.
Smart Images

Figure CN118955058A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of kerbstone processing and design, and in particular to a method for preparing kerbstones. Background Art
[0002] Curbstones refer to objects made of stone powder or concrete cast and used as boundary stones at the edge of the road surface, also known as side stones or curbstones. Curbstones are used on the road surface to distinguish the boundaries between the roadway and the sidewalk, and the green space. According to the different components, they can be divided into stone curbstones and concrete curbstones. The stone material of stone curbstones is made of natural stone with uniform texture and mechanical cutting. The strength of the stone must be qualified, and its color must be uniform, the surface must be free of cracks, the edges and corners must be complete, the appearance must be consistent, and there must be no obvious spots or color differences. Weathering is not allowed. It is not allowed to be dropped, smashed, bumped, or bumped during loading and unloading to avoid damage. Concrete curbstones refer to those made of cement and aggregate as the main raw materials, and are made by pressurization, vibration pressurization or other molding processes. Precast concrete boundary stones laid on the edge of the road surface or marking the boundary of the road surface are divided into: concrete flat curbstones with the top surface flush with the road surface, and concrete vertical curbstones with the top surface higher than the road surface.
[0003] At present, with the in-depth research on curbstone concrete at home and abroad, a curbstone preparation technology using industrial solid waste and construction waste as raw materials has emerged. For example, a full-solid waste curbstone concrete and a preparation method of a full-solid waste curbstone with publication number CN 115385647 B use industrial waste to prepare cementitious powder, and use construction waste asphalt mixture, construction waste aggregate, waste tire rubber powder and asphalt mixing plant recycled powder as aggregate, thereby realizing the recycling of industrial solid waste and construction waste, having good economy and environmental protection, complying with my country's industrial policy of energy conservation, emission reduction and green development, and having important significance for the resource utilization of industrial solid waste and construction waste.
[0004] However, the properties of industrial waste and construction waste will cause the final curbstone to be unstable or lower in strength than traditional materials. In particular, the quality and performance of waste aggregates and waste tire rubber powder are not as good as standard aggregates, affecting the durability and bearing capacity of the curbstone. Although waste recycling is of environmental significance, there are harmful components in these wastes, especially volatile organic compounds contained in waste tire rubber powder, such as benzene, toluene and xylene. These compounds will be released into the environment during the hardening or aging of concrete, which will have a negative impact on air quality. Some waste tire rubber powder even contains heavy metals such as lead, cadmium, chromium and mercury. The content of these metals is usually low, but under long-term environmental exposure, these heavy metals will gradually be released, polluting the soil and groundwater. Summary of the invention
[0005] Technical issues solved: In view of the shortcomings of the prior art, the present invention provides a method for preparing curbstones, which has the advantages that the durability of curbstones made from waste materials is close to that of standard aggregates, and the finished curbstones made from waste materials will not cause pollution, thereby solving the above-mentioned technical problems.
[0006] Technical solution: To achieve the above object, the present invention provides the following technical solution: a method for preparing a kerbstone, wherein the kerbstone formula is: high-performance ordinary silicate cement or cement mixed with nanomaterials, waste building aggregate, waste tire rubber powder, silica fume, fly ash, polymer emulsion, nanomaterials and water, and the kerbstone preparation comprises the following steps: Step 1: Treatment of waste tire rubber powder: Use chemical stabilizers: silane and siloxane to treat the waste tire rubber powder to reduce the release of volatile organic compounds and heavy metals; Step 2: Cementitious materials: Choose high-performance cement or modified cement to improve the strength and durability of concrete; Step 3: Modification of waste aggregates: Use polymer emulsion to treat waste aggregates to enhance the cohesiveness and strength of aggregates and improve the overall performance of concrete; Step 4: Add admixtures: highly reactive silica fume and fly ash to improve the performance and stability of concrete while reducing negative impacts on the environment; Step 5: Control the water-cement ratio between 0.25 and 0.35 to ensure the strength and durability of the concrete; Step 6: Mix the above materials evenly and put them into a mixer at a stirring speed of 300-500 rpm for 2-4 hours. After stirring, pour them into a mold for solidification to obtain a curbstone. The high-performance cement is cement mixed with nano materials, and the modified cement is cement mixed with active minerals.
[0007] Preferably, the silane in step one is vinyl silane: 3-aminopropyltriethoxysilane, the siloxane is polysiloxane: polydimethylsiloxane, and step one also includes a solvent and an auxiliary agent, the solvent is ethanol or deionized water for preparing a silane solution, and the auxiliary agent is a catalyst: an acidic catalyst.
[0008] Preferably, the specific steps of step 1 are: S1.1. Silane is mixed with a solvent: ethanol or water in proportion to prepare a silane solution, and siloxane is also prepared into a solution. Siloxane is usually mixed with a catalyst to form a coating solution; S1.2. Use water or air flow to wash the waste tire rubber powder to remove dust and impurities on the surface. After washing, dry the waste tire rubber powder to ensure that its humidity is less than <5%; S1.3. Put the dried waste tire rubber powder into a container and pour in the prepared silane or siloxane solution to make the waste tire rubber powder completely immersed in the solution. The soaking time is usually 15-30 minutes; S1.4, the waste tire rubber powder coated with the chemical stabilizer is evenly spread and dried. After drying, the waste tire rubber powder is baked at 60-80°C for 1-2 hours to ensure that silane and siloxane form stable chemical bonds on the surface of the waste tire rubber powder.
[0009] Preferably, the specific steps in step 2 are: S2.1. Prepare the selected cement, aggregate and admixtures, and mix them evenly in proportion in a mixer; S2.2. Put dry materials including cement, aggregates and admixtures into the mixer, start the mixer for dry mixing for 2-3 minutes, add water and continue mixing until the mixture reaches the required uniformity and workability.
[0010] Preferably, the polymer emulsion in step three is prepared by mixing one or more of polyvinyl alcohol emulsion, polypropylene emulsion, polyurethane emulsion and acrylic emulsion.
[0011] Preferably, the specific steps in step three are: S3.1. Put the dried waste aggregate into a mixer, and pour the prepared polymer emulsion into the mixer; S3.2, start the mixer and mix for 5-10 minutes to ensure that the emulsion is evenly covered on the surface of each aggregate; S3.3. Spread the treated aggregate evenly and dry it naturally, or use an oven to accelerate the drying: 70-80°C for 1-2 hours.
[0012] Preferably, the specific steps in step 4 are: S4.1. The silica fume content is 5%-10% of the total cement, and the fly ash content is 15%-30% of the total cement; S4.2. Dry mix silica fume and fly ash with cement to ensure the uniformity of the admixture and cement. Usually, a mixer is used for mixing. The mixing time is 3-5 minutes to ensure that the admixture and cement are fully mixed. S4.3. Add admixture, cement, aggregate and water into the mixer according to the formula. Mix all materials evenly in the mixer for 15-20 minutes at a speed of 60-10 rpm.
[0013] Preferably, the water-binder ratio in step 5 is defined as:
[0014] Wherein: W: the mass of water is kg; C: the mass of cement is kg; P: the mass of admixture is kg, and the admixture includes silica fume and fly ash; The target range expression is calculated as follows: Ensure that the water-cement ratio is between 0.25 and 0.35: .
[0015] Preferably, in step 5, the required water mass is calculated according to the water-binder ratio formula by using the known masses of cement and admixtures:
[0016] Where: W is the mass of water (kg); C is the mass of cement (kg); P is the mass of admixture (kg); It is the water-cement ratio, that is, the ratio of the mass of water to the total mass of cement and admixtures.
[0017] Preferably, the step five also includes strength and durability formula calculation, and the strength and durability formula is expressed as:
[0018] in: MPa is the compressive strength of concrete, which describes the ability of concrete to resist compression; is a constant of the material, which depends on the basic properties and formulation of concrete; It is a constant related to the sensitivity of water-binder ratio and usually needs to be determined through experiments.
[0019] Compared with the prior art, the present invention provides a method for preparing kerbstones, which has the following beneficial effects: 1. The present invention reduces the release of volatile organic compounds and heavy metals by treating waste tire rubber powder with silane and siloxane, forms stable chemical bonds by reacting with the surface of waste tire rubber powder by chemical stabilizers, reduces the adverse effects of waste materials on concrete performance, selects high-performance ordinary silicate cement or cement mixed with nano materials to improve the strength and durability of concrete, and nano materials improve the microstructure of cement and enhance its bonding force with other materials. Polymer emulsions: polyvinyl alcohol emulsion, polypropylene emulsion, polyurethane emulsion and acrylic emulsion are used to treat waste aggregates to enhance the bonding and strength of aggregates and improve the overall performance of concrete. The emulsion forms a protective film on the surface of aggregates to improve the adhesion and durability of aggregates, thereby achieving the beneficial effect that the durability performance of curbstones prepared using waste materials is close to that of standard aggregates.
[0020] 2. The present invention uses polymer emulsions: polyvinyl alcohol emulsion, polypropylene emulsion, to treat waste aggregates, which can enhance the cohesiveness and strength of the aggregates and form a protective film. The protective film prevents harmful substances from being released from the aggregates, reducing pollution to the environment. Assessing the strength of the concrete to ensure it meets the required durability standards ensures consistent performance of the final product, thereby reducing the risk of contamination from substandard material quality, with the beneficial effect of ensuring that the finished kerbstones made from waste materials do not produce any pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the steps of the method of the present invention; DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] See also Figure 1 , a method for preparing a curbstone, wherein the curbstone formula is: high-performance ordinary silicate cement or cement mixed with nanomaterials, waste building aggregate, waste tire rubber powder, silica fume, fly ash, polymer emulsion, nanomaterials and water, and the curbstone preparation comprises the following steps: Step 1: Treatment of waste tire rubber powder: Use chemical stabilizers: silane and siloxane to treat the waste tire rubber powder to reduce the release of volatile organic compounds and heavy metals; Step 2: Cementitious materials: Choose high-performance cement or modified cement to improve the strength and durability of concrete; Step 3: Modification of waste aggregates: Use polymer emulsion to treat waste aggregates to enhance the cohesiveness and strength of aggregates and improve the overall performance of concrete; Step 4: Add admixtures: highly reactive silica fume and fly ash to improve the performance and stability of concrete while reducing negative impacts on the environment; Step 5: Control the water-cement ratio between 0.25 and 0.35 to ensure the strength and durability of the concrete; Step 6: Mix the above materials evenly and put them into a mixer at a stirring speed of 300-500 rpm for 2-4 hours. After stirring, pour them into a mold for solidification to obtain a curbstone. The high-performance cement is cement mixed with nano materials, and the modified cement is cement mixed with active minerals.
[0024] Preferably, the silane in step one is vinyl silane: 3-aminopropyltriethoxysilane, the siloxane is polysiloxane: polydimethylsiloxane, and step one also includes a solvent and an auxiliary agent, the solvent is ethanol or deionized water for preparing a silane solution, and the auxiliary agent is a catalyst: an acidic catalyst.
[0025] Chemical stabilizer: Use silane and siloxane to treat waste tire rubber powder to reduce the release of volatile organic compounds and heavy metals. The chemical stabilizer reacts with the surface of waste tire rubber powder to form stable chemical bonds, thereby reducing the adverse effects of waste on concrete performance.
[0026] Use water washing or air flow cleaning to remove surface dust and impurities to ensure the cleanliness of the waste tire rubber powder.
[0027] After drying, the moisture content of the waste tire rubber powder is ensured to be less than 5%, preparing it for subsequent processing and mixing.
[0028] Choosing high-performance ordinary Portland cement or cement mixed with nanomaterials can significantly improve the strength and durability of concrete. Nanomaterials improve the microstructure of cement and enhance its bonding with other materials.
[0029] The use of modified cement mixed with active minerals helps to improve the properties of cement, such as better resistance to permeability and durability.
[0030] Use polymer emulsions (such as polyvinyl alcohol emulsion, polypropylene emulsion, polyurethane emulsion and acrylic emulsion) to treat waste aggregates to enhance the adhesion and strength of aggregates and improve the overall performance of concrete. The emulsion forms a protective film on the surface of aggregates to improve the adhesion and durability of aggregates.
[0031] Silica fume and fly ash as admixtures can improve the performance and stability of concrete. The admixtures can fill the pores in concrete, improve its density and durability, and reduce the negative impact on the environment.
[0032] Controlling the water-binder ratio between 0.25 and 0.35 ensures that the concrete has the proper strength and durability. A lower water-binder ratio reduces the porosity of the concrete, thereby increasing its durability and compressive strength.
[0033] Preferably, the specific steps of step 1 are: S1.1. Silane is mixed with a solvent: ethanol or water in proportion to prepare a silane solution, and siloxane is also prepared into a solution. Siloxane is usually mixed with a catalyst to form a coating solution; S1.2. Use water or air flow to wash the waste tire rubber powder to remove dust and impurities on the surface. After washing, dry the waste tire rubber powder to ensure that its humidity is less than <5%; S1.3. Put the dried waste tire rubber powder into a container and pour in the prepared silane or siloxane solution to make the waste tire rubber powder completely immersed in the solution. The soaking time is usually 15-30 minutes; S1.4, the waste tire rubber powder coated with the chemical stabilizer is evenly spread and dried. After drying, the waste tire rubber powder is baked at 60-80°C for 1-2 hours to ensure that silane and siloxane form stable chemical bonds on the surface of the waste tire rubber powder.
[0034] Preferably, the specific steps in step 2 are: S2.1. Prepare the selected cement, aggregate and admixtures, and mix them evenly in proportion in a mixer; S2.2. Put dry materials including cement, aggregates and admixtures into the mixer, start the mixer for dry mixing for 2-3 minutes, add water and continue mixing until the mixture reaches the required uniformity and workability.
[0035] Preferably, the polymer emulsion in step three is prepared by mixing one or more of polyvinyl alcohol emulsion, polypropylene emulsion, polyurethane emulsion and acrylic emulsion.
[0036] Preferably, the specific steps in step three are: S3.1. Put the dried waste aggregate into a mixer, and pour the prepared polymer emulsion into the mixer; S3.2, start the mixer and mix for 5-10 minutes to ensure that the emulsion is evenly covered on the surface of each aggregate; S3.3. Spread the treated aggregate evenly and dry it naturally, or use an oven to accelerate the drying: 70-80°C for 1-2 hours.
[0037] Preferably, the specific steps in step 4 are: S4.1. The silica fume content is 5%-10% of the total cement, and the fly ash content is 15%-30% of the total cement; S4.2. Dry mix silica fume and fly ash with cement to ensure the uniformity of the admixture and cement. Usually, a mixer is used for mixing. The mixing time is 3-5 minutes to ensure that the admixture and cement are fully mixed. S4.3. Add admixture, cement, aggregate and water into the mixer according to the formula. Mix all materials evenly in the mixer for 15-20 minutes at a speed of 60-10 rpm.
[0038] Preferably, the water-binder ratio in step 5 is defined as:
[0039] Wherein: W: the mass of water is kg; C: the mass of cement is kg; P: the mass of admixture is kg, and the admixture includes silica fume and fly ash; The target range expression is calculated as follows: Ensure that the water-cement ratio is between 0.25 and 0.35: .
[0040] Preferably, in step 5, the required water mass is calculated according to the water-binder ratio formula by using the known masses of cement and admixtures:
[0041] Where: W is the mass of water (kg); C is the mass of cement (kg); P is the mass of admixture (kg); It is the water-cement ratio, that is, the ratio of the mass of water to the total mass of cement and admixtures.
[0042] Preferably, the step five also includes strength and durability formula calculation, and the strength and durability formula is expressed as:
[0043] in: MPa is the compressive strength of concrete, which describes the ability of concrete to resist compression; is a constant of the material, which depends on the basic properties and formulation of concrete; It is a constant related to the sensitivity of water-binder ratio and usually needs to be determined through experiments.
[0044] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and alterations may be made to the embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a kerbstone, characterized in that: The formula of the kerbstone is: high-performance ordinary silicate cement or cement mixed with nanomaterials, waste construction aggregate, waste tire rubber powder, silica fume, fly ash, polymer emulsion, nanomaterials and water. The preparation of the kerbstone includes the following steps: Step 1: Treatment of waste tire rubber powder: Use chemical stabilizers: silane and siloxane to treat the waste tire rubber powder to reduce the release of volatile organic compounds and heavy metals; Step 2: Cementitious materials: Choose high-performance cement or modified cement to improve the strength and durability of concrete; Step 3: Modification of waste aggregates: Use polymer emulsion to treat waste aggregates to enhance the cohesiveness and strength of aggregates and improve the overall performance of concrete; Step 4: Add admixtures: highly reactive silica fume and fly ash to improve the performance and stability of concrete while reducing negative impacts on the environment; Step 5: Control the water-cement ratio between 0.25 and 0.35 to ensure the strength and durability of the concrete; Step 6: Mix the above materials evenly and put them into a mixer at a stirring speed of 300-500 rpm for 2-4 hours. After stirring, pour them into a mold for solidification to obtain a curbstone. The high-performance cement is cement mixed with nano materials, and the modified cement is cement mixed with active minerals.
2. The method for preparing a kerbstone according to claim 1, characterized in that: In the step 1, the silane is vinyl silane: 3-aminopropyltriethoxysilane, the siloxane is polysiloxane: polydimethylsiloxane, and the step 1 also includes a solvent and an auxiliary agent. The solvent is ethanol or deionized water for preparing a silane solution, and the auxiliary agent is a catalyst: an acidic catalyst.
3. The method for preparing a kerbstone according to claim 2, characterized in that: The specific steps of step 1 are: S1.
1. Silane is mixed with a solvent: ethanol or water in proportion to prepare a silane solution, and siloxane is also prepared into a solution. Siloxane is usually mixed with a catalyst to form a coating solution; S1.
2. Use water or air flow to wash the waste tire rubber powder to remove dust and impurities on the surface. After washing, dry the waste tire rubber powder to ensure that its humidity is less than <5%; S1.
3. Put the dried waste tire rubber powder into a container and pour in the prepared silane or siloxane solution to make the waste tire rubber powder completely immersed in the solution. The soaking time is usually 15-30 minutes; S1.4, the waste tire rubber powder coated with the chemical stabilizer is evenly spread and dried. After drying, the waste tire rubber powder is baked at 60-80°C for 1-2 hours to ensure that silane and siloxane form stable chemical bonds on the surface of the waste tire rubber powder.
4. The method for preparing a kerbstone according to claim 3, characterized in that: The specific steps in step 2 are: S2.
1. Prepare the selected cement, aggregate and admixtures, and mix them evenly in proportion in a mixer; S2.
2. Put dry materials including cement, aggregates and admixtures into the mixer, start the mixer for dry mixing for 2-3 minutes, add water and continue mixing until the mixture reaches the required uniformity and workability.
5. The method for preparing a kerbstone according to claim 4, characterized in that: In the step three, the polymer emulsion is prepared by mixing one or more of polyvinyl alcohol emulsion, polypropylene emulsion, polyurethane emulsion and acrylic emulsion.
6. The method for preparing a kerbstone according to claim 1, characterized in that: The specific steps in step three are: S3.
1. Put the dried waste aggregate into a mixer, and pour the prepared polymer emulsion into the mixer; S3.2, start the mixer and mix for 5-10 minutes to ensure that the emulsion is evenly covered on the surface of each aggregate; S3.
3. Spread the treated aggregate evenly and dry it naturally, or use an oven to accelerate the drying: 70-80°C for 1-2 hours.
7. The method for preparing a kerbstone according to claim 6, characterized in that: The specific steps in step 4 are: S4.
1. The silica fume content is 5%-10% of the total cement, and the fly ash content is 15%-30% of the total cement; S4.
2. Dry mix silica fume and fly ash with cement to ensure the uniformity of the admixture and cement. Usually, a mixer is used for mixing. The mixing time is 3-5 minutes to ensure that the admixture and cement are fully mixed. S4.
3. Add admixture, cement, aggregate and water into the mixer according to the formula. Mix all materials evenly in the mixer for 15-20 minutes at a speed of 60-10 rpm.
8. The method for preparing a kerbstone according to claim 7, characterized in that: The water-binder ratio in step 5 is defined as: Wherein: W: the mass of water is kg; C: the mass of cement is kg; P: the mass of admixture is kg, and the admixture includes silica fume and fly ash; The target range expression is calculated as follows: Ensure that the water-cement ratio is between 0.25 and 0.35: 。 9. The method for preparing a kerbstone according to claim 8, characterized in that: In step 5, the required water mass is calculated according to the water-binder ratio formula by using the known cement and admixture masses: Where: W is the mass of water (kg); C is the mass of cement (kg); P is the mass of admixture (kg); It is the water-cement ratio, that is, the ratio of the mass of water to the total mass of cement and admixtures.
10. The method for preparing a kerbstone according to claim 9, characterized in that: The step 5 also includes strength and durability formula calculation, and the strength and durability formula is expressed as: in: MPa is the compressive strength of concrete, which describes the ability of concrete to resist compression; is a constant of the material, which depends on the basic properties and formulation of concrete; It is a constant related to the sensitivity of water-binder ratio and usually needs to be determined through experiments.