Method for preparing magnesium oxychloride light partition board from activated regenerated micro powder

By activating the gelation reaction of regenerated powder with lightly burned magnesium oxide and magnesium chloride, combined with foam, expanded perlite and fiber mesh cloth, lightweight partition panels with good physical properties and chemical stability were prepared, solving traditional building materials The problems of resource depletion and poor water resistance of magnesium oxychloride cement have achieved high-value utilization of construction waste and environmentally friendly partition panel preparation.

CN118955084AActive Publication Date: 2024-11-15CHINA TIESIJU CIVIL ENGINEERING GROUP CO LTD +2

Patent Information

Application Number
CN202411061191.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The production of traditional building materials relies on a large number of natural resources to lead to resource depletion and ecological environment pollution, and the poor water resistance of magnesium oxychloride cement limits its application.

Method used

Lightweight partition panels with good physical properties and chemical stability are prepared by activating the gelation reaction of the regenerated powder with lightly calcined magnesium oxide and magnesium chloride, combined with foam, expanded perlite and fiber mesh cloth.

Benefits of technology

It realizes the high-value utilization of construction waste, reduces material costs and environmental impact, improves the strength, high temperature resistance, waterproof performance and flame retardancy of partition panels, and is suitable for the preparation of composite lightweight partition panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955084A_ABST
    Figure CN118955084A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a magnesium oxychloride light partition wall board from activated regenerated micro powder, and belongs to the technical field of partition wall board preparation. The preparation method comprises the following steps: crushing, calcining and ball-milling waste concrete to obtain regenerated micro powder, adding an alkaline activator for activation, then adding light calcined magnesia, magnesium chloride, water and boric acid, mixing with foam, and adding chopped vinylon engineering fibers to obtain slurry; and then preparing a core board from the slurry and expanded perlite, and then adding the slurry for natural curing to obtain the light partition board. According to the invention, through a specific activation process, the activity of the regenerated micro powder is improved, so that the regenerated micro powder can effectively react with a magnesium oxychloride cementing material to form a light partition board with good physical properties and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of partition board preparation, in particular to a method for preparing a magnesium oxychloride lightweight partition board by using activated regenerated micro powder. Background Art

[0002] With the acceleration of urbanization, the construction industry has developed rapidly, and a large amount of construction waste has been generated. If these wastes are not effectively treated, they will not only occupy land resources, but also cause serious pollution to the environment. On the other hand, the production of traditional building materials often relies on large-scale exploitation of natural resources, which not only aggravates the depletion of resources, but also has an adverse impact on the ecological environment. The resource utilization of construction waste has become an urgent problem to be solved. In particular, the recycled micropowder of building materials in construction waste has a certain potential activity due to its small particle size and large specific surface area. It can be converted into a material with cementitious properties through appropriate activation treatment, which can be used to replace part of cement and prepare new building materials.

[0003] Magnesium oxychloride cement is a pneumatic cement with high temperature resistance, high strength, good wear resistance and low density. Solid waste is often used as admixture in the production of magnesium oxychloride cement. The reason is that magnesium oxychloride cement has high strength and can still meet the strength requirements after adding a large amount of solid waste. The maximum admixture can reach 60%. This is the characteristic and advantage of magnesium oxychloride cement, but the disadvantage is also obvious. Magnesium oxychloride cement has poor water resistance and its hardened body will gradually lose 60-80% of its strength in water, which limits its application. Summary of the invention

[0004] In view of this, the present invention provides a method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, which improves the activity of the regenerated micropowder through a specific activation process, so that the regenerated micropowder can effectively react with the magnesium oxychloride gelling material to form a lightweight partition board with good physical properties and chemical stability. This not only realizes the high-value utilization of construction waste and reduces material costs, but also reduces the impact on the environment, and has important economic and social value.

[0005] The method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder of the present invention comprises the following steps:

[0006] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the method comprising the following steps:

[0007] S1: Preliminarily crushing the waste concrete, screening particles with a diameter of less than 40 mm, and calcining the obtained particles to obtain particles A;

[0008] S2: ball milling particle A for 2-3 hours to obtain regenerated micro powder B;

[0009] S3: calcining the regenerated micropowder B, and then mixing the regenerated micropowder with 0.1-5% by weight of an alkaline activator to obtain activated regenerated micropowder C;

[0010] S4: adding light-burned magnesium oxide and magnesium chloride to the activated regenerated micropowder C obtained in step S3, stirring continuously, then mixing with water, adding boric acid, stirring homogenously, and obtaining slurry D;

[0011] S5: mixing a foaming agent, a foam stabilizer and water to obtain foam, and then uniformly mixing slurry D and the foam to obtain slurry E;

[0012] S6: adding engineering fiber to the slurry E obtained in step S5, stirring and homogenizing to obtain slurry F;

[0013] S7: Lay a glass fiber mesh cloth in the mold, pour the slurry F obtained in step S6, then add expanded perlite, stir and homogenize, lay another layer of glass fiber mesh cloth on the shallow surface of the slurry F, and obtain the core board G after natural curing;

[0014] S8: Lay glass fiber mesh cloth flat in the mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0015] Preferably, the calcination temperature in step S1 is 300-500° C., and the calcination time is 2-3 hours.

[0016] Preferably, the diameter of the regenerated micropowder B in step S2 is 5-80 microns, and the passing rate of a 75-micron sieve is not less than 75%. The diameter of the regenerated micropowder has a great influence on the activation effect. The regenerated micropowder with a smaller diameter has a larger specific surface area and can react more effectively with the magnesium oxychloride cement raw material, thereby improving its activity.

[0017] Preferably, the alkaline activator described in step S3 is one or more of CaO, CaCl2 or Ca(OH)2.

[0018] Preferably, the calcination process in step S3 is: first calcining at a temperature of 700-800° C. for 1-3 hours, then heating to 900-1000° C. for 1-2 hours.

[0019] The calcination temperature of steps S1 and S3 has a great influence on the activation of the regenerated micropowder. High temperature thermal activation can change the mineral structure of the regenerated micropowder, promote the chemical bond breaking of the active components SiO2 and Al2O3, and generate hydration products with rehydration gelation ability, such as CSH gel.

[0020] Preferably, the mass ratio of light-burned magnesium oxide, magnesium chloride, activated regenerated micropowder C, water, and boric acid in step S4 is 120-150:30-60:80-120:100-200:5-10. Boric acid plays a retarding role, and the addition of boric acid can react with Mg during the hydration process of magnesium oxychloride cement. 2+ The ions react to form stable hydration products, which help improve the stability and strength of cement in wet environments.

[0021] Preferably, the foaming agent in step S5 is a protein foaming agent and a physical foaming agent;

[0022] The foam stabilizer is fatty acid methanol amide;

[0023] The mass ratio of the foaming agent to the foam stabilizer is 200 to 1000: 1. By adding the foam stabilizer, the foam stability in the lightweight partition board can be improved, the dispersion and uniformity in the partition board can be improved, and the strength of the partition board can be improved.

[0024] More preferably, the foaming agent is any one of rosin acid soap foaming agent, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and a composite foaming agent.

[0025] Preferably, the volume ratio of the slurry D to the foam in step S5 is 1-4:1-6.

[0026] Preferably, the engineering fiber in step S6 is chopped polyvinyl alcohol fiber with a fiber length of 5-10 mm; and the mass ratio of the slurry E to the chopped polyvinyl alcohol fiber is 300-3000:1.

[0027] Preferably, the mass ratio of the slurry F to the expanded perlite in step S7 is 3.5-5:1.

[0028] During the curing process, Ca(OH)2 and phosphoric acid in the regenerated micropowder and alkaline activator form hydroxyapatite with high waterproof performance. Silicon and aluminum in the metastable material are dissolved and polymerized through the bridging effect of sodium ions to form Si-Al-O chain polymers, forming an oligomer gel with mechanical strength.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The invention firstly calcines the regenerated micro powder, adds an alkaline activator to activate the regenerated micro powder, and then adds lightly burned magnesium oxide and magnesium chloride to further process the slurry. Since magnesium oxychloride cement is an air-hardening cement with high temperature resistance, high strength, good wear resistance and low density, it can improve the strength and high temperature resistance of the partition board. Boric acid is added to reduce the setting time of magnesium oxychloride cement, and phosphoric acid is added to participate in the generation of a compound with waterproof performance to improve the waterproof performance. Then, foam, expanded perlite and fiber mesh cloth are added to improve the integrity of the finally formed partition board and reduce the overall density of the partition board, so that a composite lightweight partition board with excellent performance can be finally prepared, and the light weight and surface density can reach 65-90kg / m 2 , has good fireproof performance. The present invention adopts expanded perlite, and the recycled micropowder and magnesium oxychloride cement used are all non-combustible and have good flame retardancy. The present invention is a magnesium oxychloride cement foamed hollow product, and there are a large number of closed tiny pores inside, which has good sound absorption and heat preservation effects, and the ultimate compressive strength is 5.0-10.0MPa, the bending load is 2-5 times, the impact resistance is greater than 5 times, and the single-point hanging force is 900-1200N. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the composition of a magnesium oxychloride lightweight partition board material prepared by using activated regenerated micropowder according to an embodiment of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments.

[0033] Example 1

[0034] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0035] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 300° C. for 2 h to obtain particles A;

[0036] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0037] S3: After calcining the regenerated micropowder B at 700°C for 1 hour, the temperature is raised to 900°C and calcined for 1 hour, and then the regenerated micropowder is fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0038] S4: 120 parts by mass of light-burned magnesium oxide and 30 parts by mass of magnesium chloride are added to 80 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 100 parts by mass of water, and 5 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0039] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 4:1 to obtain slurry E;

[0040] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 350 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0041] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, and lay another layer of glass fiber mesh cloth on the shallow surface of slurry F. After natural curing, a core board G is obtained, the thickness of the core board is 60 to 80 mm (the same below), and it is set aside;

[0042] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0043] The core material and the core board of the lightweight partition board prepared by the present invention generate micro powder hydration products and bubbles due to the reaction, which are evenly distributed in the core material and the core board. The structure of the lightweight partition board is as follows Figure 1 .

[0044] Example 2

[0045] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0046] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0047] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0048] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0049] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0050] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to dilute the mixture, and foam is obtained by a foaming machine. Slurry D and the foam are evenly mixed in a ratio of 1:5 to obtain slurry E;

[0051] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 550 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0052] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0053] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0054] Example 3

[0055] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0056] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0057] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0058] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator CaCl2 to obtain activated regenerated micropowder C.

[0059] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0060] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0061] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 550 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0062] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0063] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0064] Example 4

[0065] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0066] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0067] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0068] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0069] S4: 120 parts by mass of light-burned magnesium oxide and 30 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0070] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0071] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 500 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0072] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0073] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0074] Example 5

[0075] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0076] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0077] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0078] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0079] S4: 120 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0080] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0081] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 520 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0082] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0083] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0084] Comparative Example 1

[0085] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0086] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and obtaining particles A;

[0087] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0088] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0089] S4: 120 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0090] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0091] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 500 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0092] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0093] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0094] Comparative Example 2

[0095] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0096] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0097] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0098] S3: The regenerated micropowder is fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0099] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0100] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0101] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 550 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0102] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, and then add expanded perlite, the mass ratio of slurry F to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry F, and obtain a core board G after natural curing is completed, and set aside;

[0103] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0104] Comparative Example 3

[0105] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0106] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0107] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0108] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0109] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0110] S5: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 550 parts by mass of the slurry D obtained in step S4, and stirring and homogenizing to obtain slurry E;

[0111] S6: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry E obtained in step S5, and then add expanded perlite, the mass ratio of slurry E to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry E, and obtain a core board F after natural curing is completed, and set aside;

[0112] S7: Lay glass fiber mesh cloth in the partition board mold, pour the slurry E obtained in step S5 with a thickness of 5-10mm, place the core board G obtained in step S6 in the center of the surface of the bottom slurry E, pour the slurry E obtained in step S5 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0113] Comparative Example 4

[0114] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0115] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0116] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0117] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0118] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0119] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0120] S6: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry E obtained in step S5, and then add expanded perlite, the mass ratio of slurry E to expanded perlite is 4:1, lay another layer of glass fiber mesh cloth on the shallow surface of slurry E, and obtain a core board F after natural curing is completed, and set aside;

[0121] S7: Lay glass fiber mesh cloth in the partition board mold, pour the slurry E obtained in step S5 with a thickness of 5-10mm, place the core board F obtained in step S6 in the center of the surface of the bottom slurry E, pour the slurry E obtained in step S6 around and on the surface of the core board F, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0122] Comparative Example 5

[0123] A method for preparing a magnesium oxychloride lightweight partition board from activated regenerated micropowder, the steps are as follows:

[0124] S1: Preliminary crushing of the waste concrete by a universal crusher, screening of particles with a diameter of less than 40 mm, and calcination of the obtained particles at 500° C. for 3 h to obtain particles A;

[0125] S2: ball milling the particles A for 2 hours using a planetary ball mill to obtain regenerated micro powder B with a diameter of 5-80 μm and a passing rate of not less than 75% on a 75 μm sieve;

[0126] S3: After calcining the regenerated micropowder B at 800°C for 2 hours, the temperature is raised to 900°C and calcined for 2 hours. The regenerated micropowder is then fully mixed with 5% by weight of an alkaline activator Ca(OH)2 to obtain activated regenerated micropowder C.

[0127] S4: 150 parts by mass of light-burned magnesium oxide and 60 parts by mass of magnesium chloride are added to 120 parts by mass of activated regenerated micropowder C, and the mixture is continuously stirred, and then mixed with 200 parts by mass of water, and 8 parts by mass of boric acid are added, and the mixture is stirred and homogenized to obtain slurry D;

[0128] S5: a foaming agent (sodium dodecylbenzene sulfonate) and a foam stabilizer (fatty acid methanol amide) are mixed in a mass ratio of 500:1, and then 10 times of water is added to mix and dilute, and foam is obtained by a foaming machine, and slurry D and foam are evenly mixed in a ratio of 1:6 to obtain slurry E;

[0129] S6: adding 1 part by mass of chopped polyvinyl alcohol fibers having a fiber length of 5-10 mm to 550 parts by mass of the slurry E obtained in step S5, and stirring and homogenizing to obtain slurry F;

[0130] S7: Lay a glass fiber mesh cloth in a partition board mold, pour the slurry F obtained in step S6, lay another layer of glass fiber mesh cloth on the shallow surface of the slurry F, and obtain a core board G after natural curing, which is ready for use;

[0131] S8: Lay glass fiber mesh cloth in the partition board mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

[0132] The performance tests were conducted on the partition boards prepared in the examples and comparative examples, and the results are shown in Table 1:

[0133] Table 1

[0134]

[0135]

[0136] From Table 1 we can see that:

[0137] Analysis of the experimental results of Examples 1-2, 4-5 and Comparative Example 1 shows that in the lightweight partition board of the present invention, the regenerated micropowder needs to be pre-treated by calcination at 300-500°C first, and when the calcination time is between 2-3h, the performance of the lightweight partition board is significantly higher.

[0138] From the analysis of the experimental results of Examples 1-3 and Comparative Example 2, it can be seen that in the lightweight partition boards of the present invention, the regenerated micropowder needs to be calcined again after ball milling to improve its activity. The calcination temperature is 700-800°C, the calcination time is 1-3h, and then the temperature is raised to 900-1000°C and calcined for 1-2h, which can significantly improve the performance of the lightweight partition boards.

[0139] From the analysis of the experimental results of Examples 1-4 and Comparative Examples 3 and 4, it can be seen that the addition of foam and expanded perlite to the lightweight partition boards of the present invention can effectively reduce the surface density of the lightweight partition boards without significantly affecting the performance of the lightweight partition boards, and reduce the raw material cost of the lightweight partition boards, which has better practicality and is more conducive to the large-scale application of lightweight partition boards.

[0140] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder, characterized in that: The method comprises the following steps: S1: Preliminarily crushing the waste concrete, screening particles with a diameter of less than 40 mm, and calcining the obtained particles to obtain particles A; S2: ball milling particle A for 2-3 hours to obtain regenerated micro powder B; S3: calcining the regenerated micropowder B, and then mixing the regenerated micropowder with 0.1-5% by weight of an alkaline activator to obtain activated regenerated micropowder C; S4: adding light-burned magnesium oxide and magnesium chloride to the activated regenerated micropowder C obtained in step S3, stirring continuously, then mixing with water, adding boric acid, stirring homogenously, and obtaining slurry D; S5: mixing a foaming agent, a foam stabilizer and water to obtain foam, and then uniformly mixing slurry D and the foam to obtain slurry E; S6: adding engineering fiber to the slurry E obtained in step S5, stirring and homogenizing to obtain slurry F; S7: Lay a glass fiber mesh cloth in the mold, pour the slurry F obtained in step S6, then add expanded perlite, stir and homogenize, lay another layer of glass fiber mesh cloth on the shallow surface of the slurry F, and obtain the core board G after natural curing; S8: Lay glass fiber mesh cloth flat in the mold, pour the slurry F obtained in step S6 with a thickness of 5-10mm, place the core board G obtained in step S5 in the center of the surface of the bottom slurry F, pour the slurry F obtained in step S6 around and on the surface of the core board G, the thickness of the slurry on the core board surface is equal to the thickness of the bottom slurry, and complete natural curing to obtain a lightweight partition board.

2. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The calcination temperature in step S1 is 300-500° C., and the calcination time is 2-3 hours.

3. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The diameter of the regenerated micro powder B in step S2 is 5-80 microns, and the passing rate of the 75-micron sieve is not less than 75%.

4. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The alkaline activator described in step S3 is one or more of CaO, CaCl2 or Ca(OH)2.

5. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The calcination process in step S3 is: first at a temperature of 700-800° C. for 1-3 hours, then heating to 900-1000° C. for 1-2 hours.

6. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The mass ratio of the light-burned magnesium oxide, magnesium chloride, activated regenerated micropowder C, water and boric acid in step S4 is 120-150:30-60:80-120:100-200:5-10.

7. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The foaming agent described in step S5 is a protein foaming agent or a physical foaming agent; The foam stabilizer is fatty acid methanol amide; The mass ratio of the foaming agent to the foam stabilizing agent is 200-1000:

1.

8. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: The volume ratio of the slurry D to the foam in step S5 is 1-4:1-6.

9. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: In step S6, the engineering fiber is short-cut polyvinyl alcohol fiber with a fiber length of 5-10 mm; the mass ratio of the slurry E to the short-cut polyvinyl alcohol fiber is 300-3000:

1.

10. The method for preparing magnesium oxychloride lightweight partition board from activated regenerated micropowder according to claim 1, characterized in that: In step S7, the mass ratio of the slurry F to the expanded perlite is 3.5-5:1.

Citation Information

Patent Citations

  • Light inorganic heat insulation central layer for magnesium cement thermal insulation external wall panel and method of processing the same

    CN101492279A

  • Method for reducing hydration heat release of magnesium oxychloride cement

    CN104529204A

  • Recycled micro powder activation method

    CN106186770A

  • Silica fume filled magnesium oxychloride cement and preparation method thereof

    CN108275898A

  • Alkali residue magnesium oxychloride cement, and preparation method and application thereof

    CN111116068A

Cited By

  • High-temperature-resistant, fireproof and flame-retardant sealant as well as preparation method and application thereof