Method for preparing aerogel composite material by taking inorganic silica sol as silicon source based on initiator
Through the combination of initiator and inorganic silicone sol, the gel dipping, aging, solvent replacement and supercritical drying processes are used to solve the problems of long gel time and weak grid strength for the preparation of inorganic silicone sol, achieving high performance The preparation of silicon-based aerogel composites has good high temperature resistance and low thermal conductivity.
Patent Information
- Application Number
- CN202411020619.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the preparation of aerogel materials using inorganic silicone sol as silicon source has problems such as long gel time, weak gel grid strength, high solvent replacement cost and cumbersome process, which limits the commercial application of aerogel materials.
Combining the initiator with the inorganic silicone sol, and after stirring the alcohol solvent, the initiator, the inorganic silicone sol, water, and the catalyst, an acid or alkali-regulating solution is added to perform gel dipping, aging, solvent replacement, hydrophobic modification and supercritical Drying treatment to prepare high-performance silicon-based aerogel composite material.
Improve the stability and high temperature resistance of the aerogel network structure. The thermal conductivity of the material is less than 0.021W/mK at room temperature, less than 0.06W/mK at 500℃, and does not burn at 750℃, reducing the raw material cost and Production process complexity.
Smart Images

Figure CN118955087A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new material preparation, in particular to a method for preparing an aerogel composite material based on an initiator and taking an inorganic silica sol as a silicon source. Background Art
[0002] Silica aerogel is a lightweight porous nanomaterial with excellent thermal insulation properties. It has low density and good thermal insulation effect. It has good application prospects in aerospace, petrochemical, new energy, energy-saving buildings and other fields. At present, most aerogel materials on the market use organic silicon sources as raw materials for the production of silicon-based aerogels. The high production cost restricts the widespread application of aerogel materials. Aerogel materials prepared using inorganic silica sol as the silicon source are prepared by the sol-gel method, which has problems such as long gel time, weak gel grid strength, high solvent replacement cost, and complicated process. The large-scale production route of aerogels prepared using inorganic silicon sources needs to be further improved. Adding a small amount of initiator to the silica sol-gel system can help solve the above problems and promote the commercialization of aerogels prepared using inorganic silicon sources. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing an aerogel composite material based on an initiator and using an inorganic silica sol as a silicon source, so as to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for preparing an aerogel composite material based on an initiator using an inorganic silica sol as a silicon source, comprising the following steps:
[0005] A. Stir the alcohol solvent, initiator, inorganic silica sol, water and catalyst in a mass ratio of 1-30:0.1-1:1-50:0.1-30:0.1-1 to obtain a mixed sol solution;
[0006] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 6-8;
[0007] C. Dipping: dipping the silica sol solution into the inorganic fiber material through a dipping process to obtain a composite of the silica sol and the inorganic fiber material, and then leaving it to stand for a period of time to obtain a gel composite material;
[0008] D. Aging: adding the obtained composite gel material to an aging solution and aging at 20-60°C for 6-48h;
[0009] E. placing the obtained wet gel composite material into an alcohol solvent and performing solvent replacement 1-4 times;
[0010] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 6-24 hours;
[0011] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, and then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 2-10 hours.
[0012] Preferably, in step A, the alcohol solvent is one of methanol, ethanol or ethylene glycol, the initiator is one or more of methyl ethyl ketone peroxide, propylene oxide, 2,3-epoxypropyltrimethylammonium chloride, ethoxytrimethylsilane, dimethyldiethoxysilane, ethyl orthosilicate or tetrabutyl titanate, the inorganic silica sol is at least one of alkaline silica sol, neutral silica sol or acidic silica sol, and its mass solid content is 25-30%, and the catalyst is one or more of ammonia water, hydrofluoric acid, ammonium fluoride, ammonium fluoroborate or ammonium fluorosilicate.
[0013] Preferably, in step C, the inorganic fiber material is an inorganic fiber felt, and is made of one or more of glass fiber, ceramic fiber, pre-oxidized silk fiber, aluminum silicate fiber or rock wool fiber.
[0014] Preferably, in step D, the aging liquid is an initiator / alcohol solvent mixed solution, and the mass ratio of the initiator / alcohol solvent is 1%-100%, the initiator is one or more of methyl ethyl ketone peroxide, propylene oxide, 2,3-epoxypropyltrimethylammonium chloride, ethoxytrimethylsilane, dimethyldiethoxysilane, ethyl orthosilicate or tetrabutyl titanate, and the alcohol solvent is one of methanol, ethanol or ethylene glycol.
[0015] Preferably, in step E, the alcohol solvent is one of methanol, ethanol or ethylene glycol, and the solvent replacement time is 6-48h.
[0016] Preferably, in step F, the hydrophobic modifier is one of trimethylchlorosilane, trimethylmethoxysilane or hexamethyldisilazane.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention selects high-quality and low-cost inorganic silica sol as the inorganic silicon source material, and the raw material cost is low and the production process is simple. The inorganic gel network is initiated by an initiator to improve the stability of the aerogel network structure and the high temperature resistance of the aerogel material. At the same time, the prepared silicon-based aerogel composite material is characterized by testing. The thermal conductivity of the aerogel composite material is less than 0.021W / mK at room temperature, the thermal conductivity at a high temperature of 500°C is less than 0.06W / mK, and it does not burn at 750°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a physical picture of the prepared silica aerogel composite material. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Embodiment 1:
[0022] A. Mix alcohol solvent, initiator, inorganic silica sol, water and catalyst at a ratio of 20:0.5:15:15:
[0023] The silica sol mixture was obtained by stirring evenly with a mass ratio of 0.2;
[0024] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 6;
[0025] C. Dipping: The silica sol solution is immersed in the inorganic fiber material through the dipping process to obtain a composite of silica sol and ceramic fiber felt, and the composite material is obtained by standing for a period of time;
[0026] D. Aging: Add the obtained composite gel material into an aging solution and age it at 20°C for 6 hours;
[0027] E. placing the obtained wet gel composite material into an alcohol solvent for solvent replacement once;
[0028] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 6 hours;
[0029] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 2 hours.
[0030] Embodiment 2:
[0031] A. Stir the alcohol solvent, initiator, inorganic silica sol, water and catalyst in a mass ratio of 25:0.3:30:15:0.3 to obtain a silica sol mixed solution;
[0032] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 6.2;
[0033] C. Dipping: The silica sol solution is immersed in the inorganic fiber material through the dipping process to obtain a composite of silica sol and ceramic fiber felt, and the composite material is obtained by standing for a period of time;
[0034] D. Aging: Add the obtained composite gel material into an aging solution and age it at 30°C for 8h;
[0035] E. placing the obtained wet gel composite material into an alcohol solvent for solvent replacement twice;
[0036] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 12 hours;
[0037] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 4 hours.
[0038] Embodiment 3:
[0039] A. Stir the alcohol solvent, initiator, inorganic silica sol, water and catalyst in a mass ratio of 20:0.8:13:17:0.25 to obtain a silica sol mixed solution;
[0040] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 7;
[0041] C. Dipping: The silica sol solution is immersed in the inorganic fiber material through the dipping process to obtain a composite of silica sol and ceramic fiber felt, and the composite material is obtained by standing for a period of time;
[0042] D. Aging: Add the obtained composite gel material into an aging solution and age it at 40°C for 16h;
[0043] E. placing the obtained wet gel composite material into an alcohol solvent for solvent replacement three times;
[0044] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 18 hours;
[0045] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 8 hours.
[0046] Embodiment 4:
[0047] A. Stir the alcohol solvent, initiator, inorganic silica sol, water and catalyst in a mass ratio of 15:1:12:26:0.4 to obtain a silica sol mixed solution;
[0048] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 7.5;
[0049] C. Dipping: The silica sol solution is immersed in the inorganic fiber material through the dipping process to obtain a composite of silica sol and ceramic fiber felt, and the composite material is obtained by standing for a period of time;
[0050] D. Aging: Add the obtained composite gel material into an aging solution and age it at 50°C for 40h;
[0051] E. placing the obtained wet gel composite material into an alcohol solvent and performing solvent replacement 4 times;
[0052] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 20 hours;
[0053] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 8 hours.
[0054] Embodiment 5:
[0055] A. Stir the alcohol solvent, initiator, inorganic silica sol, water and catalyst in a mass ratio of 20:0.2:9:21:0.5 to obtain a silica sol mixed solution;
[0056] B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 8;
[0057] C. Dipping: The silica sol solution is immersed in the inorganic fiber material through the dipping process to obtain a composite of silica sol and ceramic fiber felt, and the composite material is obtained by standing for a period of time;
[0058] D. Aging: Add the obtained composite gel material into an aging solution and age it at 60°C for 48h;
[0059] E. placing the obtained wet gel composite material into an alcohol solvent and performing solvent replacement 4 times;
[0060] F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 24 hours;
[0061] G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, and then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 10 hours.
[0062] The thermal conductivity of the silicon-based aerogel composite material prepared in the embodiment is less than 0.021 W / mK at room temperature, less than 0.06 W / mK at a high temperature of 500° C., and does not burn at 750° C.
[0063] Comparative Example 1: Compared with Example 1, step A lacks an initiator, and the rest is the same as Example 1.
[0064] Comparative Example 2: Compared with Example 2, the ceramic fiber felt in step D is replaced with glass fiber felt, and the rest is the same as Example 2.
[0065] The following table shows the parameters of aerogel composite materials:
[0066]
[0067] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an aerogel composite material based on an initiator using an inorganic silica sol as a silicon source, characterized in that: The following steps are involved: A. Mix alcohol solvent, initiator, inorganic silica sol, water and catalyst in the ratio of 1-30: The mixed sol solution is obtained by stirring evenly in a mass ratio of 0.1-1:1-50:0.1-30:0.1-1; B. Add acid or alkali to the obtained mixed sol solution to adjust the pH of the solution to 6-8; C. Dipping: dipping the silica sol solution into the inorganic fiber material through a dipping process to obtain a composite of the silica sol and the inorganic fiber material, and then leaving it to stand for a period of time to obtain a gel composite material; D. Aging: adding the obtained composite gel material to an aging solution and aging at 20-60°C for 6-48h; E. placing the obtained wet gel composite material into an alcohol solvent and performing solvent replacement 1-4 times; F. Immersing the obtained wet gel composite material in a hydrophobic modifier for hydrophobic modification for 6-24 hours; G. Immerse the hydrophobically modified wet gel in an organic solvent such as methanol, ethanol or n-hexane, and then send it into a supercritical drying kettle for supercritical drying treatment, and obtain a silicon-based aerogel composite material after drying for 2-10 hours.
2. The method for preparing aerogel composite materials based on an initiator and using inorganic silica sol as a silicon source according to claim 1, characterized in that: In step A, the alcohol solvent is one of methanol, ethanol or ethylene glycol, the initiator is one or more of methyl ethyl ketone peroxide, propylene oxide, 2,3-epoxypropyltrimethylammonium chloride, ethoxytrimethylsilane, dimethyldiethoxysilane, ethyl orthosilicate or tetrabutyl titanate, the inorganic silica sol is at least one of alkaline silica sol, neutral silica sol or acidic silica sol, and its mass solid content is 25-30%, and the catalyst is one or more of ammonia water, hydrofluoric acid, ammonium fluoride, ammonium fluoroborate or ammonium fluorosilicate.
3. The method for preparing aerogel composite materials based on an initiator and using inorganic silica sol as a silicon source according to claim 1, characterized in that: In the step C, the inorganic fiber material is an inorganic fiber felt, and is made of one or more of glass fiber, ceramic fiber, pre-oxidized silk fiber, aluminum silicate fiber or rock wool fiber.
4. The method for preparing aerogel composite materials based on an initiator and using inorganic silica sol as a silicon source according to claim 1, characterized in that: In the step D, the aging liquid is an initiator / alcohol solvent mixed solution, and the mass ratio of the initiator / alcohol solvent is 1%-100%, the initiator is one or more of methyl ethyl ketone peroxide, propylene oxide, 2,3-epoxypropyltrimethylammonium chloride, ethoxytrimethylsilane, dimethyldiethoxysilane, ethyl orthosilicate or tetrabutyl titanate, and the alcohol solvent is one of methanol, ethanol or ethylene glycol.
5. The method for preparing aerogel composite materials based on an initiator and using inorganic silica sol as a silicon source according to claim 1, characterized in that: In the step E, the alcohol solvent is one of methanol, ethanol or ethylene glycol, and the solvent replacement time is 6-48 hours.
6. The method for preparing aerogel composite materials based on an initiator and using inorganic silica sol as a silicon source according to claim 1, characterized in that: In the step F, the hydrophobic modifier is one of trimethylchlorosilane, trimethylmethoxysilane or hexamethyldisilazane.
Citation Information
Cited By
Transparent aerogel as well as preparation method and application thereof
CN120271005A
A transparent aerogel and its preparation method and application
CN120271005B
Silica-based aerogel felt, flexible water-proofing and vapor-barrier silica-based aerogel composite material having ultralow thermal conductivity, and preparation method