Microwave ceramic material as well as preparation method and application thereof

CN118955108AActive Publication Date: 2024-11-15BEIJING YUAN LIU HONG YUAN ELECTRONIC TECHNOLOGY CO LTD +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411020665.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

例如中国专利CN106587987A公开了介电常数为10~20的C0G特性微波介质材料,主要是采用Ca、Sr对MgTiO3进行A位替代,从而调节介电常数和温度系数,但是该瓷料的介电常数大于10,从而限制了该材料在更高频段的应用

Benefits of technology

[0035] The low dielectric constant microwave ceramic material provided by the invention has a simple preparation process, is easy to realize mass production, has low raw material cost and is green and environmentally friendly, and can be used in the manufacture of microwave devices such as multilayer ceramic capacitors, single layer capacitors, and microwave substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967274960000021
    Figure BDA0004967274960000021
  • Figure BDA0004967274960000041
    Figure BDA0004967274960000041
  • Figure BDA0004967274960000091
    Figure BDA0004967274960000091
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic materials, and particularly relates to a microwave ceramic material and a preparation method and application thereof. The microwave ceramic material provided by the invention is prepared from the following components in percentage by mass: 77.93 to 83.84 weight percent of CaMg (Zr < 0.05 > Si < 1.95 >) O < 6 >, 11.27 to 12.12 weight percent of Sr < x > Ba < 2-x > TiSi < 2 > O < 8 >, 1.77 to 2.82 weight percent of a sintering aid and 1.77 to 9.48 weight percent of a modified additive, wherein 0 < = x < = 1.46; the sintering aid is one or more of B2O3, SiO2 and ZnO; the modified additive is one or more of a manganese compound, an aluminum compound, a cobalt compound, a niobium compound and a cerium compound. The dielectric property of the microwave dielectric ceramic material is adjusted under the combined action of the composition and dosage of each material, and the application range of the microwave dielectric ceramic material is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a microwave ceramic material and a preparation method and application thereof. Background Art

[0002] With the rapid development of 5G communication technology, high frequency is an inevitable trend in the development of microwave components. As the operating frequency of communication equipment expands to the millimeter wave band, the problem of signal delay will become more prominent, which puts higher requirements on the performance of microwave dielectric ceramics, a key material for communication equipment. Compared with medium dielectric constant materials and high dielectric constant materials, low dielectric constant materials can reduce the mutual coupling loss between the substrate and the metal electrode, and shorten the delay time of signal propagation between chips. As communication technology gradually develops in the direction of millimeter waves, the requirements for the microwave dielectric properties of chip-type multilayer ceramic capacitors MLCC are also getting higher and higher, requiring them to have a low dielectric constant (ε r <10) to improve the information transmission rate of the device, lower high-frequency dielectric loss (tanδ<0.0005) to enhance the frequency selectivity and reduce energy consumption, and near-zero frequency temperature coefficient to ensure the working stability of the signal during resonance and transmission.

[0003] At present, the research work on existing low dielectric constant materials is mainly concentrated on material systems such as Al2O3, Mg2SiO4, AWO4 (A is Ca, Sr or Ba), phosphates and R2BaCuO5 (R is Y, Sm or Yb). For example, Chinese patent CN106587987A discloses a C0G characteristic microwave dielectric material with a dielectric constant of 10 to 20, which mainly uses Ca and Sr to replace the A position of MgTiO3 to adjust the dielectric constant and temperature coefficient. However, the dielectric constant of the porcelain material is greater than 10, which limits the application of the material in higher frequency bands. Another example is Chinese patent CN111635222A discloses a high temperature sintered (1350 to 1475 ° C), low dielectric constant (ε r =6.3~6.8) of microwave dielectric material, due to the frequency stability coefficient τ of the material f =-47ppm / ℃(dielectric constant τ ε The current low dielectric constant materials have a narrow sintering temperature range, the microstructure is not dense enough, the phase control is difficult, the low dielectric constant, the high quality factor, the near-zero temperature coefficient are difficult to unify, and the anti-reduction property is poor, which limits their practical application in high-frequency components. Summary of the invention

[0004] In view of this, the present invention provides a microwave ceramic material and a preparation method and application thereof. The microwave ceramic material provided by the present invention has a controllable dielectric constant of 6.2 to 8.3 and a dielectric loss of less than 1×10 -4 , adjustable capacitance temperature coefficient (can meet CF (0 ± 15) ppm / ° C, CG (0 ± 30) ppm / ° C and AG (100 ± 30) ppm / ° C), and has a high insulation resistivity (> 1 × 10 13 Ω·cm) has expanded the application range of microwave ceramic materials.

[0005] In order to solve the above technical problems, the present invention provides a microwave ceramic material, comprising the following components in percentage by mass:

[0006]

[0007] Where 0≤x≤1.46;

[0008] The sintering aid is one or more of B2O3, SiO2 and ZnO;

[0009] The modifying additive is one or more of a manganese compound, an aluminum compound, a cobalt compound, a niobium compound and a cerium compound.

[0010] Preferably, the CaMg(Zr 0.05 Si 1.95 )O6 preparation method comprises the following steps:

[0011] CaCO3, Mg(OH)2, ZrO2 and SiO2 are first mixed and calcined to obtain the CaMg(Zr 0.05 Si 1.95 )O6.

[0012] Preferably, the first mixing is wet ball milling;

[0013] The temperature of the first calcination is 1150-1200° C., and the time is 2-5 hours.

[0014] Preferably, the Sr x Ba (2-x) The preparation method of TiSi2O8 comprises the following steps:

[0015] SrCO3, BaCO3, TiO2 and SiO2 are mixed and calcined for the second time to obtain the Sr x Ba (2-x) TiSi2O8.

[0016] Preferably, the second mixing is wet ball milling;

[0017] The second calcination is carried out at a temperature of 1100 to 1170° C. and for a time of 2 to 4 hours.

[0018] Preferably, the manganese compound is manganese oxide and / or manganese carbonate;

[0019] The aluminum compound is one or more of aluminum oxide, aluminum hydroxide and aluminum carbonate;

[0020] The cobalt compound is cobalt oxide and / or cobalt carbonate;

[0021] The niobium compound is niobium oxide and / or niobium hydroxide;

[0022] The cerium compound is cerium oxide and / or cerium carbonate.

[0023] Preferably, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, the mass percentage of each component oxide in the modifying additive to the microwave ceramic material is:

[0024] MnO 0.10~0.34wt%;

[0025] Al2O3 1.52~4.69wt%;

[0026] CoO 0.15~0.34wt%;

[0027] Nb2O5 0~3.82wt%;

[0028] CeO2 0~0.29wt%.

[0029] The present invention also provides a method for preparing the microwave ceramic material described in the above technical solution, comprising the following steps:

[0030] CaMg(Zr 0.05 Si 1.95 )O6、Sr x Ba (2-x) TiSi2O8, sintering aid and modifying additive are mixed to obtain the microwave ceramic material.

[0031] Preferably, before the mixing, the process further comprises: subjecting the sintering aid to a third calcination; the temperature of the third calcination is 550-650° C., and the time is 2-4 hours;

[0032] The mixing is wet ball milling, and the time of the wet ball milling is 5 to 10 hours.

[0033] The present invention also provides the use of the microwave ceramic material described in the above technical solution or the microwave ceramic material prepared by the method for preparing the microwave ceramic material described in the above technical solution in preparing microwave devices.

[0034] The present invention provides a microwave ceramic material, comprising the following components in percentage by weight: 77.93-83.84 wt% CaMg(Zr 0.05 Si 1.95 )O6, 11.27~12.12wt%Sr x Ba (2-x) TiSi2O8, 1.77-2.82wt% sintering aid and 1.77-9.48wt% modifier; wherein 0≤x≤1.46; the sintering aid is one or more of B2O3, SiO2 and ZnO; the modifier is one or more of manganese compound, aluminum compound, cobalt compound, niobium compound and cerium compound. 0.05 Si 1.95 )O6 microwave dielectric ceramics as the basis, by adjusting the auxiliary material (Sr x Ba (2-x) The composition and dosage of the modified additives are used to adjust the dielectric properties and microstructure of the microwave dielectric ceramic material, so that the temperature coefficient is adjustable within the temperature range of -55°C to 125°C, which meets the temperature characteristic requirements of CF (0±15) ppm / °C, CG (0±30) ppm / °C and AG (100±30) ppm / °C in GB / T 5596; and the microwave dielectric ceramic material provided by the present invention has a high insulation resistivity (>10 13 Ω·cm), which expands its application range.

[0035] The low dielectric constant microwave ceramic material provided by the present invention has a simple preparation process, is easy to realize mass production, has low raw material cost and is green and environmentally friendly, and can be used for the manufacture of microwave devices such as multilayer ceramic capacitors, single-layer capacitors, and microwave substrates. DETAILED DESCRIPTION

[0036] The present invention provides a microwave ceramic material, comprising the following components in percentage by mass:

[0037]

[0038] Where 0≤x≤1.46;

[0039] The sintering aid is one or more of B2O3, SiO2 and ZnO;

[0040] The modifying additive is one or more of a manganese compound, an aluminum compound, a cobalt compound, a niobium compound and a cerium compound.

[0041] In the present invention, unless otherwise specified, all raw materials are conventional commercial products, and the purity of all raw materials is preferably above 99%.

[0042] In terms of mass percentage, the microwave ceramic material provided by the present invention comprises 77.93-83.84 wt% CaMg(Zr 0.05 Si 1.95 )O6, preferably 79.27-83wt%, more preferably 79.46-81.65wt%. In the present invention, the CaMg(Zr 0.05 Si 1.95 )O6 preparation method preferably comprises the following steps:

[0043] CaCO3, Mg(OH)2, ZrO2 and SiO2 are first mixed and calcined to obtain the CaMg(Zr 0.05 Si 1.95 )O6.

[0044] In the present invention, the first mixing is preferably wet ball milling. The dispersant for wet ball milling is preferably water, and the water is preferably deionized water; the grinding balls for wet ball milling are preferably zirconia balls. The present invention has no special requirements for the rotation speed and time of the wet ball milling, as long as it can be mixed evenly. In the present invention, after the first mixing, it is preferred to further include: drying and sieving the first mixed product in sequence. The present invention has no special requirements for the drying, as long as the solvent can be removed. In the present invention, the aperture of the mesh screen for screening is preferably 60 to 100 mesh, more preferably 100 mesh. The present invention preferably takes the undersize for the first calcination.

[0045] In the present invention, the temperature of the first calcination is preferably 1150-1200° C., more preferably 1160-1180° C.; the time of the first calcination is preferably 2-5 hours, more preferably 3-4 hours.

[0046] In the present invention, the CaMg(Zr 0.05 Si 1.95 )O6 as the main material, the CaMg(Zr 0.05 Si 1.95 )O6 contains a small amount of Zr which can broaden the sintering temperature, stabilize the phase structure and inhibit the formation of impure phase Ca2MgSi2O7.

[0047] In terms of mass percentage, the microwave ceramic material provided by the present invention comprises 11.27-12.12 wt % Sr x Ba (2-x) TiSi2O8, preferably 11.49-12wt%. In the present invention, 0≤x≤1.46, preferably 0.16-1.44, more preferably 0.62-1.38. In the present invention, the Sr x Ba (2-x) The preparation method of TiSi2O8 preferably comprises the following steps:

[0048] SrCO3, BaCO3, TiO2 and SiO2 are mixed and calcined for the second time to obtain the Sr x Ba (2-x) TiSi2O8.

[0049] In the present invention, the second mixing is preferably wet ball milling; the dispersant for wet ball milling is preferably water, and the water is preferably deionized water; in the present invention, the material-water ratio of the wet grinding is preferably 0.8-1.2:3, more preferably 1:3; the grinding balls for wet ball milling are preferably zirconia balls. The present invention has no special requirements for the rotation speed and time of the wet ball milling, as long as it can be mixed evenly. In the present invention, when x is 0, SrCO3 is not added during the second mixing process. In the present invention, the second mixing preferably also includes: drying and sieving the second mixed product in sequence. The present invention has no special requirements for the drying, as long as the solvent can be removed. In the present invention, the aperture of the mesh screen for screening is preferably 60-100 mesh, more preferably 100 mesh. The present invention preferably takes the undersize for the second calcination.

[0050] In the present invention, the temperature of the second calcination is preferably 1100-1170° C.; the time of the second calcination is preferably 2-4 hours, more preferably 2.5-3.5 hours.

[0051] In the present invention, the Sr x Ba (2-x) As a secondary material, TiSi2O8 can improve the microstructure, increase the density, and widen the firing temperature while adjusting the capacity temperature coefficient and insulation resistance.

[0052] In terms of mass percentage, the microwave ceramic material provided by the present invention includes 1.77-2.82wt% sintering aid, preferably 2-2.46wt%. In the present invention, the sintering aid is one or more of B2O3, SiO2 and ZnO, preferably B2O3, SiO2 and ZnO. In the present invention, the sintering aid can effectively diffuse into the grain boundary layer, effectively improving the dielectric properties and porcelain strength of the microwave ceramic material; when the amount of the sintering aid added is too low, the porcelain is under-fired and the insulation resistance decreases; when the amount of the sintering aid added is too much, the dielectric loss is too large and the porcelain strength is low; the present invention limits the amount of the sintering aid to the above range to ensure the performance of the microwave ceramic material.

[0053] In terms of mass percentage, the microwave ceramic material provided by the present invention includes 1.77-9.48wt% of the modifying additive, preferably 2.27-7.97wt%, and more preferably 3.05-6.88wt%. In the present invention, the modifying additive is one or more of a manganese compound, an aluminum compound, a cobalt compound, a niobium compound, and a cerium compound. In the present invention, the manganese compound is preferably manganese oxide and / or manganese carbonate, and more preferably manganese oxide; the aluminum compound is preferably one or more of aluminum oxide, aluminum hydroxide, and aluminum carbonate, and more preferably aluminum oxide; the cobalt compound is preferably cobalt oxide and / or cobalt carbonate, and more preferably cobalt oxide; the niobium compound is preferably niobium oxide and / or niobium hydroxide, and more preferably niobium oxide; the cerium compound is preferably cerium oxide and / or cerium carbonate, and more preferably cerium oxide. In the present invention, the manganese oxide is preferably MnO, the aluminum oxide is preferably Al2O3, the cobalt oxide is preferably CoO, the niobium oxide is preferably Nb2O5, and the cerium oxide is preferably CeO2.

[0054] In the present invention, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, based on the total mass of the microwave ceramic material, the modifying additive preferably includes 0.10-0.34wt% MnO, more preferably 0.23-0.33wt%, and further preferably 0.25-0.29wt%. In the present invention, the additive MnO can ensure that the microwave device (capacitor) has a lower dielectric loss under microwaves and improve the Q value of the capacitor. The present invention limits the amount of manganese oxide to the above range to maintain the performance of the microwave device well. Too little addition will increase the dielectric loss of the microwave device under microwaves, and the microwave device is prone to heat failure. Too much addition will result in a loose porcelain structure and poor dielectric properties.

[0055] In the present invention, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, based on the total mass of the microwave ceramic material, the modifying additive preferably includes 1.52-4.69wt% Al2O3, more preferably 2.39-3.83wt%, and further preferably 2.45-2.5wt%. In the present invention, the additive Al2O3 can improve the sintering characteristics of the ceramic body, enhance the mechanical strength of the ceramic body, and improve the dielectric properties. The present invention limits the amount of alumina to the above range to maintain the performance of the ceramic performance well. If the amount is too little, the mechanical strength is poor and the dielectric loss is high. If the amount is too much, the ceramic body is difficult to sinter.

[0056] In the present invention, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, based on the total mass of the microwave ceramic material, the modifying additive preferably includes 0.15-0.34wt% CoO, more preferably 0.23-0.25wt%. In the present invention, the additive CoO can improve and increase the insulation resistance of the capacitor and effectively reduce the dielectric loss. If the addition amount is too low, it is not conducive to improving the insulation resistance of the microwave device; if the addition amount is too much, it makes the microwave device difficult to sinter.

[0057] In the present invention, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, based on the total mass of the microwave ceramic material, the modifying additive preferably includes 0-3.82wt% Nb2O5, more preferably 1.23-3.35wt%, and further preferably 1.47-2.82wt%. In the present invention, the additive Nb2O5 can increase the lattice activity of the powder, facilitate sintering, and improve the reliability of the ceramic capacitor.

[0058] In the present invention, when the modifying additive is MnO, Al2O3, CoO, Nb2O5 and CeO2, based on the total mass of the microwave ceramic material, the modifying additive preferably includes 0-0.29wt% CeO2, more preferably 0.1-0.25wt%. In the present invention, the additive CeO2 can prevent the aging of the capacitor, refine the grains, and ensure the dielectric properties of the capacitor.

[0059] The present invention also provides a method for preparing the microwave ceramic material described in the above technical solution, comprising the following steps:

[0060] CaMg(Zr 0.05 Si 1.95 )O6、Sr x Ba (2-x) TiSi2O8, sintering aid and modifying additive are mixed to obtain the microwave ceramic material.

[0061] In the present invention, the mixing preferably further comprises: subjecting the sintering aid to a third calcination. In the present invention, the third calcination preferably further comprises: subjecting one or more of B2O3, SiO2 and ZnO to wet ball milling and then drying and sieving in sequence. In the present invention, the dispersant for wet ball milling is preferably water, and the water is preferably deionized water; the grinding balls for wet ball milling are preferably zirconia balls; the rotation speed of the wet balls is preferably 300-400r / min, more preferably 350r / min; the wet ball milling time is preferably 4-6h, more preferably 5h. In the present invention, the drying temperature is preferably 60-80°C, more preferably 70°C. The present invention has no special requirements for the drying time, as long as the solvent can be removed. In the present invention, the aperture of the sieve for sieving is preferably 100 mesh. The present invention preferably takes the undersize for the third calcination.

[0062] In the present invention, the temperature of the third calcination is preferably 550-650°C, more preferably 600-630°C; the time of the third calcination is preferably 2-4h, more preferably 2.5-3.5h. The present invention can remove the carbon dioxide and / or crystal water adsorbed in the sintering aid component through the third calcination. In the present invention, the sintering aid is a low melting point substance that can promote the sintering of the porcelain body.

[0063] In the present invention, the mixing is preferably wet ball milling; the dispersant for wet ball milling is preferably water, and the water is preferably deionized water; the grinding balls for wet ball milling are preferably zirconia balls; the time of wet ball milling is preferably 5 to 10 hours, more preferably 6 to 8 hours. In the present invention, after the mixing, it is preferred to further include: drying and sieving the mixed materials in sequence. In the present invention, the drying temperature is preferably 110 to 130°C, more preferably 120°C; the drying time is preferably 5 to 7 hours, more preferably 6 hours. In the present invention, the aperture of the sieve for sieving is preferably 100 mesh.

[0064] The present invention also provides the use of the microwave ceramic material described in the above technical solution or the microwave ceramic material prepared by the preparation method of the microwave ceramic material described in the above technical solution in preparing a microwave device. In the present invention, the microwave device preferably includes a ceramic capacitor or a substrate.

[0065] In the present invention, the method for preparing a microwave device using a microwave ceramic material preferably comprises the following steps:

[0066] The microwave ceramic material and the binder are mixed and then granulated and molded in sequence to obtain a green body;

[0067] The green body is sequentially debinded and sintered to obtain the microwave device.

[0068] In the present invention, the binder is preferably a polyvinyl butyral solution, and the mass concentration of the polyvinyl butyral solution is preferably 10%. The present invention has no special limitation on the granulation, and a conventional method in the art can be used. In the present invention, the molding pressure is preferably 4 to 6 MPa. In the present invention, the shape of the blank is preferably a disc or a cylinder.

[0069] In the present invention, the debinding temperature is preferably 440-460°C, more preferably 450°C; the debinding holding time is preferably 2.5-3.5h, more preferably 3h. In the present invention, the heating rate to the temperature required for debinding is preferably 3°C / min. In the present invention, the sintering temperature is preferably 1240-1340°C, more preferably 1270-1300°C; the sintering holding time is preferably 2-5h, more preferably 3-4h.

[0070] In the present invention, after the sintering, the process preferably further comprises: cooling the sintered product to room temperature in the furnace. In the present invention, the room temperature is preferably 20-35°C, more preferably 25-30°C.

[0071] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0072] Example 1

[0073] CaCO3, Mg(OH)2, ZrO2, SiO2 with a purity of 99% were mixed into CaMg(Zr 0.05 Si 1.95 )O6 in a planetary ball mill at a speed of 350 r / min for 5 h. The wet ball milled product was dried at 120 ° C and passed through a 60-mesh sieve. The sieve was calcined at 1170 ° C for 3 h to obtain CaMg(Zr 0.05 Si 1.95 )O6;

[0074] The preparation method of Ba2TiSi2O8 preferably comprises the following steps:

[0075] BaCO3, TiO2, SiO2 (the molar ratio of BaCO3, TiO2 and SiO2 is 2:1:2) with a purity of 99% and deionized water are mixed in a mass ratio of the total mass of BaCO3, TiO2 and SiO2 to the mass of the dispersant of 1:3, and then wet-grinded (using zirconia balls as grinding balls), the wet-grinded product is dried and passed through a 60-mesh sieve, and the sieve is calcined at 1170°C for 3h to obtain Ba2TiSi2O8;

[0076] B2O3, SiO2 and ZnO with a purity of 99% were mixed in a molar ratio of 3:2:5 in a planetary ball mill at a speed of 350 r / min (using deionized water as solvent and zirconium balls as grinding balls) for 5 hours, then dried at 70°C, sieved through a 100-mesh sieve, and calcined at 600°C for 4 hours to obtain a sintering aid;

[0077] CaMg(Zr 0.05 Si 1.95 )O6, Ba2TiSi2O8, sintering aids and modification additives according to CaMg(Zr 0.05 Si 1.95 )O6 has a mass percentage of 83%, Ba2TiSi2O8 has a mass percentage of 12%, a sintering aid has a mass percentage of 2%, and a modifying additive has a mass percentage of 3% (including 0.25% MnO, 2.5% Al2O3, and 0.25% CoO) and is placed in a planetary ball mill with deionized water as a dispersant and zirconia balls as grinding balls, and wet-milled for 5 hours, followed by drying at 120°C for 6 hours. The mixture is sieved with a sieve with an aperture of 100 meshes to obtain a microwave ceramic material.

[0078] Embodiments 2 to 20

[0079] The microwave ceramic material was prepared according to the method of Example 1, except that Sr with different x values ​​was prepared with reference to Table 1. x Ba (2-x) TiSi2O8, refer to Table 2 to limit CaMg(Zr 0.05 Si 1.95 )O6、Sr x Ba (2-x) Composition and mass percentage of TiSi2O8, sintering aids and modifying additives.

[0080] Table 1 Sr x Ba (2-x) Formula design and calcination temperature of TiSi2O8

[0081]

[0082]

[0083] Table 2 Formula design content of microwave ceramic materials prepared in Examples 1 to 20 (mass percentage / wt%)

[0084]

[0085]

[0086] Test of dielectric properties: The microwave ceramic material and PVB (polyvinyl butyral) solution with a mass concentration of 10wt% were mixed and granulated, and then pressed into discs and cylindrical green bodies at a pressure of 4Mpa and 6MPa respectively, and the temperature was raised to 450℃ at a heating rate of 3℃ / min for debinding for 3h; the green body after debinding was sintered at 1270℃ for 3h, and naturally cooled to room temperature (25℃) in the furnace; the two surfaces of the fired discs were coated with silver paste, silver electrodes were fired, and the room temperature electrical properties of the capacitors were tested. The results are listed in Table 3.

[0087] Table 3 Performance parameters of products obtained by porcelain material formula

[0088]

[0089]

[0090] Note: The capacitance, dielectric loss and insulation resistivity of the samples related to the dielectric constant are all tested at room temperature 25℃±3℃.

[0091] It can be seen from Table 3 that the relative dielectric constant of the microwave device prepared by the microwave ceramic material provided by the present invention is 6.19-8.25, and the temperature coefficient (CF, CG, AG) of the high-frequency capacitor ceramic material is met in the range of -55℃ to 125℃, and the insulation resistivity is greater than 1×10 13 Ω·cm.

[0092] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A microwave ceramic material, It is characterized in that Includes the following components in percentage by mass: Where 0≤x≤1.46; The sintering aid is B 2 O 3 、SiO 2 and one or more of ZnO; The modifying additive is one or more of a manganese compound, an aluminum compound, a cobalt compound, a niobium compound and a cerium compound.

2. The microwave ceramic material according to claim 1, It is characterized in that The CaMg(Zr 0.05 Si 1.95 ) 6 The preparation method comprises the following steps: CaCO 3 Mg(OH) 2 、ZrO 2 and SiO 2 The first mixing is performed by the first calcination to obtain the CaMg(Zr 0.05 Si 1.95 ) 6 .

3. The microwave ceramic material according to claim 2, It is characterized in that The first mixing is wet ball milling; The temperature of the first calcination is 1150-1200° C., and the time is 2-5 hours.

4. The microwave ceramic material according to claim 1, It is characterized in that The Sr x Ba (2-x) TiS 2 O 8 The preparation method comprises the following steps: SrCO 3 、BaCO 3 、TiO 2 and SiO 2 The second mixing is carried out for the second calcination to obtain the Sr x Ba (2-x) TiS 2 O 8 .

5. The microwave ceramic material according to claim 4, It is characterized in that The second mixing is wet ball milling; The second calcination is carried out at a temperature of 1100 to 1170° C. and for a time of 2 to 4 hours.

6. The microwave ceramic material according to claim 1, It is characterized in that The manganese compound is manganese oxide and / or manganese carbonate; The aluminum compound is one or more of aluminum oxide, aluminum hydroxide and aluminum carbonate; The cobalt compound is cobalt oxide and / or cobalt carbonate; The niobium compound is niobium oxide and / or niobium hydroxide; The cerium compound is cerium oxide and / or cerium carbonate.

7. The microwave ceramic material according to claim 6, It is characterized in that When the modifying additive is MnO, Al 2 O 3 、CoO、Nb 2 O 5 and CeO 2 The mass percentage of each component oxide in the modified additive in the microwave ceramic material is: MnO 0.10~0.34wt%; <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 1.52~4.69wt%; CoO 0.15~0.34wt%; Nb 2 O 5 0~3.82wt%; CeO 2 0~0.29wt%。 8. The method for preparing the microwave ceramic material according to any one of claims 1 to 7, It is characterized in that The following steps are involved: CaMg(Zr 0.05 Si 1.95 ) 6 , Sr x Ba (2-x) TiS 2 O 8 , a sintering aid and a modifying additive are mixed to obtain the microwave ceramic material.

9. The method for preparing the microwave ceramic material according to claim 8, It is characterized in that Before the mixing, the method further comprises: performing a third calcination on the sintering aid; the temperature of the third calcination is 550-650° C. and the time is 2-4 hours; The mixing is wet ball milling, and the time of the wet ball milling is 5 to 10 hours.

10. Use of the microwave ceramic material according to any one of claims 1 to 7 or the microwave ceramic material prepared by the method for preparing the microwave ceramic material according to claim 8 or 9 in preparing microwave devices.

Citation Information

Patent Citations

  • Dielectric adjustable microwave ceramic dielectric material and method of producing the same

    CN101492294A

  • Low-dielectric constant microwave ceramic dielectric material and preparation method thereof

    CN102659396A

  • Microwave dielectric ceramic material with low dielectric constant and preparation method thereof

    CN106587968A

  • C0G microwave dielectric material, preparation method thereof, and preparation method of ceramic material

    CN106587987A

  • Ceramic dielectric material for high-capacity and high-voltage MLCC (multilayer ceramic capacitors) and method for preparing ceramic dielectric material

    CN107500754A