Low-temperature sintered ceramic material with high compactness and ultralow loss and preparation method thereof

CN118955129AActive Publication Date: 2024-11-15ZHAOQING UNIV
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410880734.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

[0003]但是在目前的微波介质陶瓷材料制备过程中制备方法温度高,介电性能不佳;如申请号为CN202310912232.3的中国专利公开了一种镍离子掺杂调控低介磷酸镁微波介质陶瓷及制备方法,通过控制Ni元素对Mg元素的摩尔取代量制备了一系列(Mg1-xNix)3(PO4)2低介磷酸盐微波介质材料,显著改善了Mg3(PO4)2陶瓷的微波介电性能,但是烧结温度超过1000℃,介电性能仍不能满足需求;申请号为CN202410238529.0的中国专利公开了一种复合离子掺杂优化低介高Q硅酸盐微波介质陶瓷及制备方法,其烧结温度仍然高于1000℃,相对介电常数小于10

Benefits of technology

[0026] (1) The present invention provides a low-temperature sintered ceramic material with high density and ultra-low loss, and its composition expression is (La 1-x Nd x ) 2 (Zr 0.96 Ti 0.04 ) 3 (MoO 4 ) 9 , when X is 0.5 in the formula, the relative dielectric constant (ε r ) reached 10.44, Q×f=149962GHz, τ f =-34.8ppm/℃, density up to 3.9g/cm 3 .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955129A_ABST
    Figure CN118955129A_ABST
Patent Text Reader

Abstract

The invention provides a low-temperature sintered ceramic material with high compactness and ultralow loss and a preparation method of the low-temperature sintered ceramic material, and belongs to the field of microwave dielectric ceramic materials. The composition expression of the microwave dielectric ceramic material prepared by the invention is (La1-xNdx) 2 (Zr0. 96Ti0. 04) 3 (MoO4) 9, and X in the formula is 0.1-0.7. The relative dielectric constant (epsilon r) of the ceramic material reaches 10.44, Q * f is equal to 149962GHz, tau f is equal to-34.8 ppm / DEG C, and the density can reach 3.9 g / cm < 3 >. The preparation method is simple, the sintering temperature is 650-800 DEG C, the preparation time is short, and the preparation method is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of microwave dielectric ceramic materials, and in particular relates to a low-temperature sintered ceramic material with high density and ultra-low loss and a preparation method thereof. Background Art

[0002] With the continuous innovation of communication technology, the requirements for the performance of microwave components are becoming increasingly stringent, and the characteristics of miniaturization, lightness, high frequency, and low power consumption have attracted much attention. The integration of multi-layer chip components not only reduces the size of the equipment and reduces the cost, but also enables low-temperature co-firing with low-loss metal electrodes. Therefore, low relative dielectric constant (ε r <20) and low temperature (<960℃) microwave dielectric ceramics have become the research focus, and LTCC technology has attracted much attention in the industry.

[0003] However, in the current preparation process of microwave dielectric ceramic materials, the preparation method has high temperature and poor dielectric properties. For example, the Chinese patent application number CN202310912232.3 discloses a nickel ion doped low-dielectric magnesium phosphate microwave dielectric ceramic and a preparation method, and a series of (Mg 1-x Ni x )3(PO4)2 low dielectric phosphate microwave dielectric material significantly improves the microwave dielectric properties of Mg3(PO4)2 ceramics, but the sintering temperature exceeds 1000℃, and the dielectric properties still cannot meet the requirements; Chinese patent application number CN202410238529.0 discloses a composite ion doped optimized low dielectric high Q silicate microwave dielectric ceramic and preparation method, whose sintering temperature is still higher than 1000℃, and the relative dielectric constant is less than 10. Moreover, the existing microwave dielectric ceramic materials have not improved their density, so there is an urgent need for a microwave dielectric ceramic material with high density and ultra-low loss, and a simple preparation process and low sintering temperature. Summary of the invention

[0004] In view of this, the present invention aims to provide a low-temperature sintered ceramic material with high density and ultra-low loss and a preparation method thereof, wherein the relative dielectric constant (ε r ) reached 10.44, Q×f=149962GHz, τ f =-34.82ppm / ℃, and the sintering temperature during preparation is only 650-800℃.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] In the first aspect, the present invention provides a low-temperature sintered ceramic material with high density and ultra-low loss, the composition expression of which is (La 1-x Ndx )2(Zr 0.96 Ti 0.04 )3(MoO4)9, wherein X is 0.1-0.7.

[0007] As a preference, (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 where X is 0.3-0.7.

[0008] More preferably, (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 where X is 0.5.

[0009] By adopting the above technical solution, it is proved by experiments that when X is 0.5, the (La 0.5 Nd 0.5 )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramics, which have remarkable dielectric properties.

[0010] In a second aspect, the present invention provides a method for preparing the above-mentioned low temperature sintered ceramic material, comprising the following steps:

[0011] 1) According to (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 stoichiometric ratio of La2O3, Nd2O3, ZrO2, TiO2 and MoO3 are weighed and mixed to obtain a mixed raw material powder;

[0012] 2) subjecting the mixed raw material powder of step 1) to first ball milling, first drying, sieving, pre-calcining, second ball milling, and second drying to obtain pre-treated raw material powder;

[0013] 3) Mixing the pretreated raw material powder in step 2) with a binder, pressing and molding, removing the binder, and sintering to obtain a low-temperature sintered ceramic material with high density and ultra-low loss.

[0014] Preferably, in step 1), the particle sizes of La2O3, Nd2O3, ZrO2, TiO2 and MoO3 are 350-400 mesh, and the purities are 99.99%, 99.99%, 99.99%, 99.9% and 99.99% respectively.

[0015] Preferably, the first ball milling and the second ball milling in step 2) are both carried out in a deionized water medium for 23.5-24 hours.

[0016] Preferably, the temperature of the first drying and the second drying in step 2) is 90-95°C.

[0017] Preferably, the sieving mesh number in step 2) is 40 meshes.

[0018] Preferably, the pre-sintering temperature in step 2) is 600° C. and the pre-sintering time is 2 h.

[0019] Preferably, in step 3), the mass ratio of the pretreated raw material powder to the adhesive is 1:0.05.

[0020] More preferably, the adhesive in step 3) is polyvinyl alcohol.

[0021] Preferably, the shape of the pressed product in step 3) is a cylindrical block with a height and a diameter of 5.5 mm and 12 mm respectively.

[0022] Preferably, the method for removing the adhesive in step 3) is to keep the temperature at 500° C. for 4 hours.

[0023] Preferably, in step 3), the sintering temperature is 650° C.-800° C., and the sintering time is 4 hours.

[0024] More preferably, the sintering temperature in step 3) is 725-775°C, and the most preferred sintering temperature is 750°C. By adopting the above technical solution, the present invention finds that by controlling the temperature and Nd 3+ The appropriate amount of substitution promotes densification. The reduction of pores and the increase of grain size increase the apparent density of the sample, because the dense structure and moderate grain growth can fill the space more effectively, giving it a high Q×f value.

[0025] Contains at least the following beneficial technical effects:

[0026] (1) The present invention provides a low-temperature sintered ceramic material with high density and ultra-low loss, the composition expression of which is (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9, where X is 0.5, the relative dielectric constant (ε r ) reached 10.44, Q×f=149962GHz, τ f =-34.8ppm / ℃, density can reach 3.9g / cm 3 .

[0027] (2) The preparation method of the present invention is simple, the sintering temperature is 650-800°C, the preparation time is short, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0029] Figure 1 XRD patterns of the ceramic materials prepared in Examples 1-4 at a sintering temperature of 750° C. and an enlarged view of the characteristic peak (119);

[0030] Figure 2 The scanning electron microscope (SEM) images of the ceramic materials prepared in Examples 1-4 sintered at 750° C. and the corresponding grain size distribution diagrams;

[0031] Figure 3 At different sintering temperatures (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 density variation diagram of ceramic material;

[0032] Figure 4 for (La 1-x Nd x )2(Zr 0.96 Ti 0.04 Scanning electron microscope (SEM) images of )3(MoO4)9 ceramic material obtained in different sintering temperature ranges when x=0.5 and their corresponding grain size distribution diagrams. DETAILED DESCRIPTION

[0033] The present invention will be described in detail below by specific examples. These examples are provided in order to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. The test methods in the following examples, unless otherwise specified, are conventional methods. Unless otherwise specified, the reagents and materials used can all be obtained through commercial channels.

[0034] Example 1

[0035] Preparation (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic materials

[0036] 1) According to the expression (La 1-x Nd x )2(Zr 0.96Ti 0.04 )3(MoO4)9, where X is 0.1, weigh out 400 meshes of La2O3, Nd2O3, ZrO2, TiO2, and MoO3 powders with purities of 99.99%, 99.99%, 99.99%, 99.99%, and 99.99% respectively, and mix them into a ball mill;

[0037] 2) The mixed raw material powders of step 1) are respectively ball-milled for 24 hours with deionized water as the medium, then dried at 95° C., passed through a 40-mesh sieve, and pre-calcined at 600° C. for 2 hours; after the pre-calcination, the mixed raw material powders are ball-milled for 24 hours with deionized water as the medium, and then dried at 95° C. to obtain pre-treated raw material powders;

[0038] 3) The pretreated raw material powders of step 2) were mixed with polyvinyl alcohol in a mass ratio of 1:0.05, and then pressed into cylindrical blocks with a height and diameter of 5.5 mm and 12 mm respectively, and then kept at 500° C. for 4 h to remove the adhesive;

[0039] Then the ceramic material was sintered at 750°C for 4 hours.

[0040] like Figure 1 As shown in Figure 2, when x = 0.1, all the diffraction peaks observed in the spectrum are consistent with the phase of La2Zr3(MoO4)9 (PDF#00-052-0688). This clearly confirms that the prepared ceramic material is a one-dimensional crystal phase in the sample with (167) triclinic phase structure of space group. Figure 1 (a) shows the changes of the entire XRD diffraction pattern in detail, while Figure 1 (b) amplifies the change of the 119 characteristic peak. As the x content increases, due to the Nd 3+ The ionic radius is smaller than that of La 3+ , resulting in a tighter crystal structure, which causes the 119 characteristic diffraction peak in the XRD spectrum to shift to the right. This shift phenomenon is consistent with the Bragg diffraction law, that is, changes in unit cell parameters and volume will directly affect the position of the diffraction peak in the XRD spectrum.

[0041] Figure 2 (a1) is the SEM image of the ceramic in this example. It can be seen that the sample is sintered densely and the average grain size is 1.654μm.

[0042] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 9.63, 82621GHz, and -36.4ppm / ℃ respectively.

[0043] Example 2

[0044] Preparation (La1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic material, wherein X is 0.3, and the preparation method is the same as Example 1.

[0045] like Figure 1 As shown in Figure 2, when x = 0.3, all the diffraction peaks observed in the spectrum are consistent with the phase of La2Zr3(MoO4)9 (PDF#00-052-0688). This clearly confirms that the prepared ceramic material is a one-dimensional crystal phase in the sample with (167) triclinic phase structure of space group.

[0046] Figure 2 (b1) is the SEM image of the ceramic in this example. It can be seen that the sample is sintered densely and the average grain size is 1.725μm.

[0047] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 10.21, 100671 GHz, and -33 ppm / ℃ respectively.

[0048] Example 3

[0049] Preparation (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic material, wherein X is 0.5, and the preparation method is the same as Example 1.

[0050] like Figure 1 As shown in Figure 2, when x = 0.5, all the diffraction peaks observed in the spectrum are consistent with the phase of La2Zr3(MoO4)9 (PDF#00-052-0688). This clearly confirms that the prepared ceramic material is a one-dimensional crystal phase in the sample with (167) triclinic phase structure of space group.

[0051] Figure 2 (c1) is the SEM image of the ceramic in this example. It can be seen that the sample is sintered densely and the average grain size is 1.571μm.

[0052] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 10.44, 149962GHz, and -34.8ppm / ℃ respectively.

[0053] Example 4

[0054] Preparation (La 1-x Ndx )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic material, wherein X is 0.7, and the preparation method is the same as Example 1.

[0055] like Figure 1 As shown in Figure 2, when x = 0.7, all the diffraction peaks observed in the spectrum are consistent with the phase of La2Zr3(MoO4)9 (PDF#00-052-0688). This clearly confirms that the prepared ceramic material is a one-dimensional crystal phase in the sample with (167) triclinic phase structure of space group.

[0056] Figure 2 (d1) is the SEM image of the ceramic in this example. It can be seen that the sample is sintered densely and the average grain size is 1.619 μm.

[0057] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 10.35, 111135GHz, and -39.7ppm / ℃ respectively.

[0058] Example 5

[0059] Preparation (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic materials

[0060] 1) According to the expression (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9, where X is 0.1, weigh out 350 mesh La2O3, Nd2O3, ZrO2, TiO2, and MoO3 powders with purities of 99.99%, 99.99%, 99.99%, 99.99%, and 99.99% respectively, and mix them into a ball mill;

[0061] 2) The mixed raw material powders of step 1) are respectively subjected to ball milling for 23.5-24 hours with deionized water as the medium, and then dried at 90° C., passed through a 40-mesh sieve, and pre-calcined at 600° C. for 2 hours; after the pre-calcination, the mixed raw material powders are subjected to ball milling for 23.5 hours with deionized water as the medium, and then dried at 90° C. to obtain pre-treated raw material powders;

[0062] 3) The pretreated raw material powders of step 2) were mixed with polyvinyl alcohol in a mass ratio of 1:0.05, and then pressed into cylindrical blocks with a height and diameter of 5.5 mm and 12 mm respectively, and then kept at 500° C. for 4 h to remove the adhesive;

[0063] Then the ceramic material was sintered at 750°C for 4 hours.

[0064] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 9.05, 72145GHz, and -33.9ppm / ℃ respectively.

[0065] Example 6

[0066] Preparation (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 ceramic materials

[0067] 1) According to the expression (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9, where X is 0.1, weigh out 375 meshes of La2O3, Nd2O3, ZrO2, TiO2, and MoO3 powders with purities of 99.99%, 99.99%, 99.99%, 99.99%, and 99.99% respectively, and mix them into a ball mill;

[0068] 2) The mixed raw material powders of step 1) are respectively ball-milled for 24 hours with deionized water as the medium, then dried at 93° C., passed through a 40-mesh sieve, and pre-calcined at 600° C. for 2 hours; after the pre-calcination, the mixed raw material powders are ball-milled for 24 hours with deionized water as the medium, and then dried at 93° C. to obtain pre-treated raw material powders;

[0069] 3) The pretreated raw material powders of step 2) were mixed with polyvinyl alcohol in a mass ratio of 1:0.05, and then pressed into cylindrical blocks with a height and diameter of 5.5 mm and 12 mm respectively, and then kept at 500° C. for 4 h to remove the adhesive;

[0070] Then the ceramic material was sintered at 750°C for 4 hours.

[0071] The ε of the microwave dielectric ceramic material prepared in this example r , Q×f value and τ f They are 9.22, 77779 GHz, and -35.7 ppm / ℃ respectively.

[0072] Example 7

[0073] Referring to the preparation method of Example 1, the (La1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9, X=(0.1, 0.3, 0.5, 0.7) ceramic materials were subjected to density and SEM analysis.

[0074] like Figure 3 As shown in Figure 2, the apparent density of the sample increases at 650℃-750℃ and decreases at 750℃-800℃. The increase at 650℃-750℃ may be related to the reduction of pores, while the decrease at 750℃-800℃ may be related to the abnormal growth of grains. At 750℃, the material reaches the best density, indicating that Nd 3+ The appropriate amount of substitution promotes the densification of ceramics.

[0075] like Figure 4 As shown, Figure 4 (a) to (g) show (La 1-x Nd x )2(Zr 0.96 Ti 0.04 Scanning electron microscope (SEM) images of the )3(MoO4)9 sample at x = 0.5, obtained in the sintering temperature range of 650℃ to 800℃ and the corresponding grain size distribution diagram. These images not only reveal the characteristics of the material's microstructure, but also show the morphology and size changes of the grains at different sintering temperatures. Figure 4 (a) to Figure 4 (g) shows the microstructural changes of the samples at different sintering temperatures. Figure 4 (a) and Figure 4 In (b), we can see that there are obvious pores in the sample and the grain size is small. This microstructure directly affects the apparent density of the sample, making it relatively low in density. As the sintering temperature gradually increases, Figure 4 (c) and Figure 4 (d) At the beginning, the number of pores decreased significantly and the sample surface gradually became dense. When the sintering temperature reached 750℃ (e.g. Figure 4 (e) shows that the grain size becomes more uniform and the surface structure is very dense. However, when the sintering temperature is further increased, as shown in Figure 4 (f) and Figure 4 As shown in (g), the grain growth gradually becomes non-uniform, which may have some adverse effects on the microwave dielectric properties of the ceramic.

[0076] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A low-temperature sintered ceramic material with high density and ultra-low loss, characterized in that: Its composition expression is (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9, wherein X is 0.1-0.

7.

2. The method for preparing a low temperature sintered ceramic material according to claim 1, characterized in that: The following steps are involved: 1) According to (La 1-x Nd x )2(Zr 0.96 Ti 0.04 )3(MoO4)9 stoichiometric ratio of La2O3, Nd2O3, ZrO2, TiO2 and MoO3 are weighed and mixed to obtain a mixed raw material powder; 2) subjecting the mixed raw material powder of step 1) to first ball milling, first drying, sieving, pre-calcining, second ball milling, and second drying to obtain pre-treated raw material powder; 3) Mixing the pretreated raw material powder in step 2) with a binder, pressing and molding, removing the binder, and sintering to obtain a low-temperature sintered ceramic material with high density and ultra-low loss.

3. The preparation method according to claim 2, characterized in that: In the step 1), the particle sizes of La2O3, Nd2O3, ZrO2, TiO2 and MoO3 are 350-400 meshes, and the purities are 99.99%, 99.99%, 99.99%, 99.9% and 99.99% respectively.

4. The preparation method according to claim 2, characterized in that: In the step 2), the first ball milling and the second ball milling are both carried out in a deionized water medium for 23.5-24 hours.

5. The preparation method according to claim 2, characterized in that: In the step 2), the first drying and the second drying temperatures are both 90-95°C.

6. The preparation method according to claim 2, characterized in that: The mesh size of the sieve in step 2) is 35-40 meshes.

7. The preparation method according to claim 2, characterized in that: In the step 2), the pre-firing temperature is 600° C. and the time is 2 hours.

8. The preparation method according to claim 2, characterized in that: In the step 3), the mass ratio of the pretreated raw material powder to the adhesive is 1:0.05; the adhesive is polyvinyl alcohol.

9. The preparation method according to claim 2, characterized in that: The method for removing the adhesive in step 3) is to keep the temperature at 500° C. for 4 hours.

10. The preparation method according to claim 2, characterized in that: In the step 3), the sintering temperature is 650° C.-800° C., and the sintering time is 4 hours.

Citation Information

Patent Citations

  • Nickel ion doping regulation low-dielectric magnesium phosphate microwave dielectric ceramic and preparation method thereof

    CN116924789A

  • Composite ion doped optimized low-dielectric high-Q silicate microwave dielectric ceramic and preparation method thereof

    CN118125816A

  • Manufacturing technology of molybdenum-based rare-earth alloy slab and equipment thereof

    CN101423911A

  • Molybdenum base low-temperature sintered microwave medium ceramic material

    CN101891476A

  • Lanthanum molybdate-based intermediate-temperature solid oxide fuel cell electrolyte material and preparation method thereof