High-configuration-entropy sodium niobate-based lead-free dielectric energy storage ceramic material as well as preparation method and application thereof
By introducing high configuration entropy design and using MnO2 additives in sodium niobate-based ceramics, the phase change problem of NaNbO3-based ceramics under the action of electric field is solved, and its relaxation characteristics and energy storage density are significantly improved, achieving high efficiency Improved energy storage performance.
Patent Information
- Application Number
- CN202411020841.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The existing NaNbO3-based ceramics have irreversible phase transitions under the action of electric fields, resulting in large leakage conductance and loss under high fields, limiting the improvement of their energy storage performance.
Introduce a high configuration entropy design of Na(1-0.5x)Bi0.5x(Nb(1-x)Fe0.2xZr0.2xTi0.2xHf0.2xTa0.2x)O3 in sodium niobate-based ceramics, and use a small amount of MnO2 As a sintering aid, the relaxation and sintering characteristics of the ceramic are regulated.
It significantly improves the relaxation characteristics and energy storage density of sodium niobate-based ceramics, improves the breakdown electric field and energy storage efficiency, and makes its performance close to or exceeds that of commercial lead-based ceramic capacitors.
Smart Images

Figure CN118955131A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of dielectric materials, and in particular relates to a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method and application thereof. Background Art
[0002] Materials, information and energy are the three pillars of current scientific and technological development, and together they form the foundation of modern high technology. As a cross-field, dielectric ceramic capacitors are widely used in important fields such as pulsed lasers, electronic circuits, new energy vehicles, and aerospace due to their fast charging and discharging rates, high power density, high mechanical strength, excellent stability, and good safety. Among them, lead-based ceramic capacitors occupy the dominant position in the ceramic dielectric capacitor market with their excellent energy storage performance and discharge characteristics, but the harm of lead to the environment and health is an issue that needs to be addressed urgently.
[0003] Ferroelectric materials based on perovskite lead-free ceramics have become a hot topic in the current research of dielectric materials, such as BaTiO3 (BT), SrTiO3 (ST), Bi 0.5 Na 0.5 TiO3(BNT), NaNbO3(NN), K 0.5 Na 0.5 NbO3 (KNN). Among them, NaNbO3 ceramics have attracted extensive attention in the field of dielectric energy storage due to their high Curie temperature, large bandgap, good modulatability, multi-phase transition and other characteristics, as well as their low density, which meets the current application of electronic information products for lightweight, miniaturization and integration. However, the free energy levels of the room temperature antiferroelectric Pbma phase (P phase) and the metastable ferroelectric P21ma phase (Q phase) of pure NaNbO3 ceramics are very close. Under the action of an electric field, the P phase will irreversibly transform into the Q phase, thus showing a square saturation hysteresis loop with ferroelectric characteristics, resulting in large leakage conductance and loss under high fields, making it impossible to obtain a high breakdown electric field and efficiency, limiting the improvement of the energy storage performance of NaNbO3-based ceramics. To this end, researchers have adopted a variety of methods to solve the problem of low energy storage performance of sodium niobate-based ceramics, among which the high configuration entropy strategy is an effective way to improve the energy storage performance of NaNbO3-based ceramics. For example, the Chinese patent (publication number CN115991599A) introduces high-component Bi (Zn) into NaNbO3-based ceramics. 0.2 Mg 0.2 A1 0.2 Mn 0.2 Hf 0.2 )O3, successfully prepared entropy-increasing perovskite oxide-doped ceramics, but its energy storage properties are still far from practical application. In addition, the Chinese patent (publication number: CN114956809A) by 0.2 Bi0.2 Ba 0.2 Sr 0.2 Ca 0.2 ) TiO3 and NaNbO3 composites increase the energy storage density of ceramics to 3.51 J / cm 3 Therefore, the development of new entropy-increased NaNbO3-based ceramic capacitors is of great value in the further development and application of capacitors. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and its preparation method and application, and to improve the relaxation properties of sodium niobate-based ceramics through a high configuration entropy strategy to provide a new lead-free NaNbO3-based ceramic capacitor with high energy storage characteristics.
[0005] The method can significantly improve the relaxation characteristics of sodium niobate-based lead-free energy storage ceramics, obtain high energy storage density and efficiency, and improve the breakdown resistance of ceramics. The ceramics obtained by the present invention have high breakdown field strength and excellent energy storage performance, and the preparation process is simple, the sample uniformity is good, the reliability is high, and it is lead-free and pollution-free. It is a new generation of electronic ceramic materials that conforms to the national material development strategy.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The present invention introduces for the first time into sodium niobate-based ceramics
[0008] Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3 high configuration entropy design, by introducing Fe, Zr, Ti, Hf, Ta with the same molar fraction to replace Nb at the B position to construct high entropy components
[0009] Bi 0.5 Na 0.5 (Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x)O3 is used to adjust the relaxation characteristics of the ceramics, and a small amount of MnO2 is used as a sintering aid to improve the sintering characteristics of sodium niobate-based ceramics and reduce their leakage conduction. The relaxation characteristics of sodium niobate-based ceramic materials are significantly improved, while the loss is reduced, the energy storage efficiency and the breakdown electric field are improved, and the energy storage density of sodium niobate-based lead-free dielectric energy storage ceramics is significantly improved, which is not inferior to the current commercial lead-based ceramic capacitor materials, and has important application value.
[0010] The first aspect of the present invention provides a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material, the chemical composition of the dielectric energy storage ceramic material is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+ywt%MnO2, where 0.1<x≤0.30, 0.4≤y≤0.5.
[0011] Preferably, x=0.15, 0.20, 0.25, 0.30.
[0012] More preferably, x=0.20, 0.25.
[0013] As a preferred embodiment of the present invention, the mass fraction of MnO2 is 0.4%.
[0014] The second aspect of the present invention provides a method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material, comprising the following steps:
[0015] S1: Na2CO3, Bi2O3, Nb2O5, Fe2O3, ZrO2, TiO2, HfO2, Ta2O5 and MnO2 are selected as raw materials;
[0016] S2: According to Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+y wt%MnO2 in a stoichiometric ratio (other raw materials except MnO2, MnO2 is mixed in a subsequent step) to obtain a batch, and ball-milling and mixing uniformly to obtain a batch after ball milling, wherein 0.1<x≤0.30, 0.4≤y≤0.5;
[0017] S3: calcining the ingredients after ball milling in step S2 to obtain pre-sintered raw material powder;
[0018] S4: ball-milling the pre-sintered raw material powder in step S3 for the second time, drying and then passing through a 200-mesh sieve to obtain a second-milled raw material powder;
[0019] It should be noted that the drying in S4 is a common operation in the art, such as drying at 100-120°C.
[0020] S5: performing secondary calcination on the raw material powder obtained by secondary ball milling in step S4 to obtain secondary pre-sintered raw material powder;
[0021] S6: adding MnO2 to the raw material powder pre-sintered twice in step S5 and performing ball milling three times, followed by drying and then passing through a 200-mesh sieve to obtain raw material powder of sodium niobate-based lead-free dielectric energy storage ceramic material;
[0022] It should be noted that the tape casting process in S6 is a common operation in this field.
[0023] S7: adding an organic solvent, an emulsifier, a plasticizer, a binder and a dispersant to the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S6 and mixing them evenly to obtain a slurry of the sodium niobate-based lead-free dielectric energy storage ceramic material;
[0024] S8: preparing a ceramic film of corresponding components from the slurry of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S7 through a tape casting process, and then cutting and isostatic pressing the slurry to obtain a green body of the sodium niobate-based lead-free dielectric energy storage ceramic material;
[0025] S9: performing a debinding process on the green body of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S8 to obtain a debinded ceramic material;
[0026] S10: Sintering the ceramic material after debinding in step S9 to obtain a sodium niobate-based dielectric energy storage ceramic material, namely, the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material.
[0027] Furthermore, in step S2, the specific conditions for the first ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 20-23h.
[0028] Furthermore, in step S4, the specific conditions of the secondary ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 10-15h.
[0029] Furthermore, in step S6, the specific conditions of the three ball millings are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 10-15h.
[0030] As a preferred embodiment of the present invention, the specific conditions for the first ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials (ingredients) is 2.5:1.5:1, the ball milling speed is 430r / min, and the ball milling time is 22h.
[0031] As a preferred embodiment of the present invention, the specific conditions of secondary ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials (pre-sintered raw material powder) is 2.5:1.5:1, the ball milling speed is 430r / min, and the ball milling time is 12h.
[0032] As a preferred embodiment of the present invention, the specific conditions of the three ball millings are: anhydrous ethanol and ZrO2 balls are used as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials (a mixture of secondary pre-sintered raw material powder and MnO2) is 2.5:1.5:1, the ball milling speed is 430r / min, and the ball milling time is 12h.
[0033] Furthermore, in step S3, the specific conditions of the calcination are: calcination at 800-900° C. for 4-6 hours under closed conditions.
[0034] Furthermore, in step S5, the specific conditions of the secondary calcination are: calcining at 850° C. for 5 hours under closed conditions.
[0035] As a preferred embodiment of the present invention, in step S3, the specific conditions of calcination are: calcination at 800-850°C for 4-6h under closed conditions, more preferably, calcination at 850°C for 5h under closed conditions.
[0036] As a preferred embodiment of the present invention, in step S5, the specific conditions of the secondary calcination are: calcination at 800-850°C for 4-6h under closed conditions, more preferably, calcination at 850°C for 5h under closed conditions.
[0037] Furthermore, in step S6, the amount of MnO2 added is 0.4-0.5% of the sum of the mass of the ingredients in step S2 and the amount of MnO2 added.
[0038] Further, in step S7, the organic solvent is a mixture of anhydrous ethanol and butanone, wherein the amount of anhydrous ethanol added is 50-55% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material, and the amount of butanone added is 100-105% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the emulsifier is triolein, and the amount of triolein added is 2.8-3.2% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; The plasticizer is dibutyl phthalate, and the added amount of dibutyl phthalate is 2.8-3.2% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the binder is polyvinyl butyral, and the added amount of polyvinyl butyral is 10-12% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the dispersant is polyethylene glycol, and the added amount of polyethylene glycol is 2.8-3.2% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material.
[0039] As a preferred embodiment of the present invention, in step S7, the amount of anhydrous ethanol added is 50% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material, the amount of butanone added is 105% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of triolein added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of dibutyl phthalate added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of polyvinyl butyral added is 11% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; and the amount of polyethylene glycol added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material.
[0040] Furthermore, in step S6, the specific conditions of the isostatic pressing treatment are: temperature 70-80°C, and pressurization pressures of 50MPa, 100MPa, 150MPa and 200MPa respectively.
[0041] As a preferred embodiment of the present invention, in step S6, the specific conditions of the isostatic pressing treatment are: temperature 80°C, and pressurizing pressures of 50 MPa, 100 MPa, 150 MPa and 200 MPa respectively.
[0042] Furthermore, in step S6, the specific conditions of the isostatic pressing treatment are: temperature 70-80°C, pressurization pressures of 50MPa, 100MPa, 150MPa and 200MPa respectively, and each level of pressurization time is 30min.
[0043] Further, in S9, the debinding treatment is carried out at 500-700°C for 12-24h.
[0044] As a preferred embodiment of the present invention, in step S9, the debinding treatment is carried out at 550-600°C for 20-22 hours. More preferably, the debinding treatment is carried out at 600°C for 20 hours.
[0045] Further, in step S10, the sintering conditions are: in a closed condition, the temperature is raised from room temperature to 1100-1300°C at a heating rate of 1.5-3.5°C / min and kept at that temperature for 2-6 hours, and then naturally cooled to room temperature in the furnace.
[0046] As a preferred embodiment of the present invention, in step S10, the sintering conditions are: under closed conditions, the temperature is increased from room temperature to 1100-1300°C at a heating rate of 1.5-3.5°C / min and kept warm for 2-6 hours, and then naturally cooled to room temperature with the furnace. More preferably, under closed conditions, the temperature is increased from room temperature to 1180°C at a heating rate of 2°C / min and kept warm for 5 hours.
[0047] The third aspect of the present invention provides an application of a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material, which is used as an energy storage material in the fields of laser, integrated circuit, electronic information or aerospace.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] (1) The lead-free energy storage ceramic prepared by the present invention has good relaxation characteristics, excellent energy storage density and efficiency, and high ceramic breakdown resistance. In addition, it has a simple preparation process, good sample uniformity, high reliability, and is lead-free and pollution-free. It is a new generation of electronic ceramic materials that conforms to the national material development strategy.
[0050] (2) The present invention adopts a Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3 is designed with high configuration entropy to regulate the relaxation characteristics of NaNbO3-based ceramics, and a small amount of MnO2 is selected as a sintering aid to improve the sintering characteristics of sodium niobate-based ceramics and reduce their leakage conductance. While significantly improving the relaxation characteristics of sodium niobate-based ceramic materials, the loss of ceramics is reduced, the energy storage efficiency and breakdown electric field are improved, and the energy storage density of sodium niobate-based lead-free dielectric energy storage ceramics is significantly improved. This high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material is no less than the currently commercial lead-based ceramic capacitor material and has great practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1The following are X-ray diffraction patterns of various embodiments and comparative examples.
[0052] Figure 2 is the configuration entropy calculated for the examples and comparative examples.
[0053] Figure 3 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 1.
[0054] Figure 4 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 2.
[0055] Figure 5 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Comparative Example 1.
[0056] Figure 6 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Comparative Example 2.
[0057] Figure 7 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 3.
[0058] Figure 8 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 4. DETAILED DESCRIPTION
[0059] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0060] The component models, material names, connection structures, control methods and other features not clearly described in the present invention are all regarded as common technical features disclosed in the prior art. The molecular formula of the high-configuration entropy sodium niobate-based dielectric energy storage ceramic in the present invention is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4-0.5wt%MnO2. Wherein, x=0-0.30. Preferably, x=0.20, x=0.25. In the present invention, the obtained sodium niobate-based dielectric ceramic has excellent energy storage performance. For x=0.20, the maximum breakdown electric field reaches 1060kV / cm, and the energy storage density is 12.68J / cm 3, the energy storage efficiency is 85.1%; for x = 0.25, the maximum breakdown electric field is 1060 kV / cm, and the energy storage density is 11.81 J / cm 3 , the energy storage efficiency is 85.1%.
[0061] The high configuration entropy sodium niobate-based dielectric ceramic prepared by the present invention has excellent energy storage performance, good reliability and simple process flow. The sodium niobate-based dielectric energy storage ceramic provided by the present invention and its preparation method are exemplarily described below.
[0062] In the following examples and comparative examples, polyvinyl butyral was purchased from Aladdin Reagents, with a molecular weight of 295.83; polyethylene glycol was purchased from Aladdin Reagents.
[0063] Example 1
[0064] This embodiment provides a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2, where x=0.20.
[0065] The specific preparation method is as follows:
[0066] (1) Selecting Na2CO3, Bi2O3, Nb2O5, Fe2O3, ZrO2, TiO2, HfO2, Ta2O5 and MnO2 with a purity greater than 99% as raw materials for sodium niobate-based lead-free dielectric energy storage ceramic materials;
[0067] (2) According to Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2 in a stoichiometric ratio (wherein x=0.20) are weighed as raw materials, and are evenly mixed through a ball milling process (other raw materials except MnO2, MnO2 will be mixed in a subsequent step) to obtain initial raw material powders (ingredients after ball milling); wherein anhydrous ethanol and ZrO2 balls are used as ball milling media during ball milling, the mass ratio of ZrO2 balls to raw materials is 2.5:1, the mass ratio of anhydrous ethanol to raw materials is 1.5:1, the rotation speed of the ball mill is 430r / min, and the ball milling time is 20h to obtain the ingredients after ball milling.
[0068] (3) calcining the dried and ball-milled ingredients at 850° C. for 5 h under closed conditions to obtain a pre-synthesized ceramic powder (pre-sintered raw material powder);
[0069] (4) ball milling the pre-synthesized ceramic powder, and drying the milled slurry at 100° C.; wherein anhydrous ethanol and ZrO2 balls are used as ball milling media, the mass ratio of ZrO2 balls to raw materials is 2.5:1, the mass ratio of anhydrous ethanol to raw materials is 1.5:1, the speed of the ball mill is 430 r / min, and the ball milling time is 12 h;
[0070] (5) drying the product obtained in step (4) and passing it through a 200-mesh sieve to obtain a raw material powder of a secondary ball-milled sodium niobate-based lead-free dielectric energy storage ceramic material (secondary ball-milled raw material powder);
[0071] (6) calcining the raw powder of the ceramic material in step (5) at 850° C. for 5 h under closed conditions to obtain a secondary sintered ceramic powder (secondary pre-sintered raw powder);
[0072] (7) adding 0.4 wt% MnO2 to the secondary sintered ceramic powder and ball milling, drying the ball-milled slurry at 100°C and then passing it through a 200-mesh sieve to obtain a raw material powder of a sodium niobate-based lead-free dielectric energy storage ceramic material; wherein anhydrous ethanol and ZrO2 balls are used as ball milling media during ball milling, the mass ratio of ZrO2 balls to raw materials is 2.5:1, the mass ratio of anhydrous ethanol to raw materials is 1.5:1, the rotation speed of the ball mill is 430 r / min, and the ball milling time is 12 h;
[0073] (8) The raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material is uniformly mixed with an organic solvent, an emulsifier, a plasticizer, a binder and a dispersant to obtain a slurry of the sodium niobate-based lead-free dielectric energy storage ceramic material. The organic solvent is a mixture of anhydrous ethanol and butanone; the emulsifier is triolein; the plasticizer is dibutyl phthalate; the binder is polyvinyl butyral; and the dispersant is polyethylene glycol. The amount of anhydrous ethanol added is 55% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of butanone added is 105% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of triolein added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of polyvinyl butyral added is 10% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of polyethylene glycol added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of dibutyl phthalate added is 3% of the mass of the raw powder of the sodium niobate-based lead-free dielectric energy storage ceramic material;
[0074] (9) preparing the obtained sodium niobate-based lead-free dielectric energy storage ceramic material slurry into a ceramic film through a tape casting process, and then cutting it into 10 mm×10 mm square pieces, and pressurizing it at 80° C. using pressures of 50 MPa, 100 MPa, 150 MPa, and 200 MPa in sequence, each level of pressurization for 30 minutes, to obtain a sodium niobate-based lead-free dielectric energy storage ceramic material green body;
[0075] (10) The obtained sodium niobate-based lead-free dielectric energy storage ceramic material green body is kept at 600°C for 20 hours for debinding treatment, and then the ceramic body after debinding is heated to 1180°C at a heating rate of 2°C / min under closed conditions and kept for 5 hours, and finally cooled to room temperature in the furnace to obtain the sodium niobate-based lead-free dielectric energy storage ceramic material, which is the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material.
[0076] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Example 1 is shown. It can be seen that the obtained Example ceramic has no obvious impurities. The configuration entropy S of the perovskite ceramic can be calculated by the following formula:
[0077]
[0078] Where R is the ideal gas constant, N / M is the number of cations / anions, and x is the atomic content. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. It can be seen that the configuration entropy of sodium niobate-based ceramics gradually increases with the increase of x value. The two sides of the obtained sodium niobate-based lead-free dielectric energy storage ceramic material are plated with gold electrodes by ion sputtering. The hysteresis loop of the material is tested at room temperature and 10Hz using a ferroelectric test system (Precision Premier II, USA). Its energy storage characteristics can be calculated by the following formula:
[0079]
[0080] Where W tot Represents the total energy storage density, W rec Represents the releasable energy density (energy storage density), W loss represents the energy loss density. P is the polarization intensity, P max is the maximum polarization intensity, P r is the residual polarization intensity and η is the energy storage efficiency. Figure 3 The hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 1 was measured at room temperature and 10 Hz. As can be seen from the figure, the hysteresis loop of the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material prepared by the present invention is slender, with a high breakdown electric field strength, and the maximum electric field strength (BDS) can reach 1060 kV / cm. Figure 3 It can be found that W tot and W rec It increases rapidly with the increase of electric field strength. When the electric field strength reaches 1060kV / cm, W tot =14.90J / cm 3 , W rec =12.68J / cm 3 , the corresponding η is 85.12%.
[0081] Example 2
[0082] This embodiment provides a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2, where x=0.25.
[0083] The preparation method in this example is similar to that in Example 1, except that step (2) is changed to: (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2(wherein x=0.25).
[0084] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Example 2 is shown. It can be seen that the obtained Example ceramic has no obvious impurities. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. It can be seen that the configuration entropy of sodium niobate-based ceramics gradually increases with the increase of x value. Figure 4 The hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 2 was measured at room temperature and 10 Hz. As can be seen from the figure, the hysteresis loop of the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material prepared by the present invention is slender, with a high breakdown electric field strength, and the maximum electric field strength can reach 1060 kV / cm. When the electric field strength reaches 1060 kV / cm, W tot =13.33J / cm 3 , W rec =11.87J / cm 3, the corresponding η is 89.06%.
[0085] Comparative Example 1
[0086] This comparative example provides a sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2, where x=0.
[0087] The preparation method in this comparative example is similar to that in Example 1, except that step (2) is changed to: (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2 (wherein x=0.00); and the calcination temperature in (10) is changed from 1180°C to 1300°C (as the high entropy component increases, the entropy value of the system increases, and the ceramic is easier to sinter into porcelain, so the sintering temperature in this comparative example is higher).
[0088] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Comparative Example 1 is shown. It can be seen that the obtained example ceramic has no obvious impurities. Figure 5 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Comparative Example 1 measured at room temperature and 10 Hz. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. Figure 2 and Figure 5 It can be found that the sodium niobate-based dielectric energy storage ceramic W that has not been improved by the entropy increase strategy tot and W rec Low, and loss W loss When the electric field strength reaches 360kV / cm, the ceramic is broken down. tot =3.35J / cm 3 , W rec =0.77J / cm 3 , the corresponding η is 23.00%.
[0089] Comparative Example 2
[0090] This comparative example provides a sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2, where x=0.
[0091] The preparation method in this comparative example is similar to that in Example 1, except that step (2) is changed to: (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2(wherein x=0.10).
[0092] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Comparative Example 2 is shown. It can be seen that the obtained example ceramic has no obvious impurities. Figure 6 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Comparative Example 2 measured at room temperature and 10 Hz. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. Figure 2 and Figure 6 It can be found that when x = 0.10, the low configuration entropy sodium niobate-based dielectric energy storage ceramic W tot and W rec Low, and loss W loss When the electric field strength reaches 540kV / cm, the ceramic is broken down. tot =7.04J / cm 3 , W rec =3.26J / cm 3 , the corresponding η is 46.30%.
[0093] Example 3
[0094] This embodiment provides a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2xTa 0.2x )O3+0.4wt%MnO2, where x=0.15.
[0095] The preparation method in this example is similar to that in Example 1, except that step (2) is changed to: (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2(wherein x=0.15).
[0096] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Example 3 is shown. It can be seen that the obtained Example ceramic has no obvious impurities. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. It can be seen that the configuration entropy of sodium niobate-based ceramics gradually increases with the increase of x value. Figure 7 The hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 3 was measured at room temperature and 10 Hz. As can be seen from the figure, the hysteresis loop of the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material prepared by the present invention is slender, with a high breakdown electric field strength, and the maximum electric field strength can reach 720 kV / cm. It can be found from the figure that W tot and W rec As the electric field strength increases, W loss As the electric field strength increases, it increases slowly. When the electric field strength reaches 720 kV / cm, W tot =9.80J / cm 3 , W rec =7.40J / cm 3 The corresponding η is 75.48%.
[0097] Example 4
[0098] This embodiment provides a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material and a preparation method thereof, wherein the ceramic chemical composition is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2, where x=0.30.
[0099] The preparation method in this example is similar to that in Example 1, except that step (2) is changed to: (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+0.4wt%MnO2(wherein x=0.30).
[0100] The prepared sodium niobate-based lead-free dielectric energy storage ceramics were subjected to X-ray diffraction test. Figure 1 The X-ray diffraction pattern of Example 4 is shown. It can be seen that the obtained Example ceramic has no obvious impurities. Figure 8 This is the hysteresis loop of the sodium niobate-based lead-free dielectric energy storage ceramic material prepared in Example 4 measured at room temperature and 10 Hz. Figure 2 The configuration entropy of sodium niobate-based dielectric energy storage ceramics is shown. It can be seen that the configuration entropy of sodium niobate-based ceramics gradually increases with the increase of x value. Figure 2 and Figure 8 It can be seen from the figure that the hysteresis loop of the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material prepared by the present invention is slender, the breakdown electric field strength is high, and the maximum electric field strength can reach 900kV / cm. tot and W rec As the electric field strength increases, it increases rapidly. When the electric field strength reaches 900 kV / cm, W tot =10.60J / cm 3 , W rec =9.58J / cm 3 , the corresponding η is 90.32%.
[0101] Depend on Figure 1 It can be seen that Comparative Example 1, Comparative Example 2, Example 1, Example 2, Example 3 and Example 4 are all stable perovskite phases without obvious secondary phases. Comparative Examples 1 and Comparative Examples 2 show multiple peaks of the P phase at room temperature, and Examples 1, Example 2, Example 3 and Example 4 transform from the P phase to the R phase (Pbnm phase). Figure 2 The configuration entropy values of Comparative Examples 1 and 2 and Examples 1, 2, 3 and 4 are shown. As the x value increases, the peak shape of the entire X-ray diffraction spectrum shifts to the left, indicating that the introduction of the high entropy component causes the lattice expansion.
[0102] Figure 3-8These are the unipolar ferroelectric test curves of comparative examples 1 and 2 and embodiments 1, 2, 3 and 4. It can be seen that the relaxation performance of the sodium niobate-based energy storage ceramics is significantly improved with the addition of high entropy components, and the overall breakdown strength is significantly improved with the doping of high entropy components, reaching the highest breakdown field strength of 1060 kV / cm for x=0.20 and x=0.25; due to the improvement of relaxation performance, the efficiency increases from 23.00% when x=0 to 90.32% when x=0.30.
[0103] The maximum breakdown field strength of both Example 1 and Example 2 of the present invention is 1060 kV / cm, and the maximum W rec 12.68 J / cm 3 , 11.87J / cm 3 , the efficiencies are 85.12% and 89.06% respectively.
[0104] Table 1 shows the energy storage performance of sodium niobate-based dielectric energy storage ceramics in the embodiments and comparative examples of the present invention.
[0105]
[0106]
[0107] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material, characterized in that: The chemical composition of the dielectric energy storage ceramic material is Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+ywt%MnO2, where 0.1<x≤0.30, 0.4≤y≤0.
5.
2. A method for preparing the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material as claimed in claim 1, characterized in that: The following steps are involved: S1: Na2CO3, Bi2O3, Nb2O5, Fe2O3, ZrO2, TiO2, HfO2, Ta2O5 and MnO2 are selected as raw materials; S2: According to Na (1-0.5x) Bi 0.5x (Nb (1-x) Fe 0.2x Zr 0.2x Ti 0.2x Hf 0.2x Ta 0.2x )O3+y wt%MnO2 in a stoichiometric ratio to obtain a batch, and once ball-milling and mixing to obtain a batch after ball milling, wherein 0.1<x≤0.30, 0.4≤y≤0.5; S3: calcining the ingredients after ball milling in step S2 to obtain pre-sintered raw material powder; S4: ball-milling the pre-sintered raw material powder in step S3 for the second time, drying and then passing through a 200-mesh sieve to obtain a second-milled raw material powder; S5: performing secondary calcination on the raw material powder obtained by secondary ball milling in step S4 to obtain secondary pre-sintered raw material powder; S6: adding MnO2 to the raw material powder pre-sintered twice in step S5 and performing ball milling three times, followed by drying and then passing through a 200-mesh sieve to obtain raw material powder of sodium niobate-based lead-free dielectric energy storage ceramic material; S7: adding an organic solvent, an emulsifier, a plasticizer, a binder and a dispersant to the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S6 and mixing them evenly to obtain a slurry of the sodium niobate-based lead-free dielectric energy storage ceramic material; S8: preparing a ceramic film of corresponding components from the slurry of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S7 through a tape casting process, and then cutting and isostatic pressing the slurry to obtain a green body of the sodium niobate-based lead-free dielectric energy storage ceramic material; S9: performing a debinding process on the green body of the sodium niobate-based lead-free dielectric energy storage ceramic material described in step S8 to obtain a debinded ceramic material; S10: Sintering the ceramic material after debinding in step S9 to obtain a sodium niobate-based dielectric energy storage ceramic material, namely, the high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material.
3. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S2, the specific conditions of the first ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 20-23h; In step S4, the specific conditions of the secondary ball milling are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 10-15h; In step S6, the specific conditions of the three ball millings are: using anhydrous ethanol and ZrO2 balls as ball milling media, the mass ratio of ZrO2 balls, anhydrous ethanol and raw materials is (2.2-2.6):(1.4-1.6):1, the ball milling speed is 420-460r / min, and the ball milling time is 10-15h.
4. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S3, the specific conditions of calcination are: calcination at 800-900° C. for 4-6 hours under closed conditions; In step S5, the specific conditions of the secondary calcination are: calcination at 800-900° C. for 4-6 hours in a closed condition.
5. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S6, the amount of MnO2 added is 0.4-0.5% of the sum of the mass of the ingredients in step S2 and the amount of MnO2 added.
6. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S7, the organic solvent is a mixture of anhydrous ethanol and butanone, wherein the amount of anhydrous ethanol added is 50-55% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; the amount of butanone added is 100-105% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; The emulsifier is triolein, and the amount of triolein added is 2.8-3.2% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; The plasticizer is dibutyl phthalate, and the amount of dibutyl phthalate added is 2.8-3.2% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; The binder is polyvinyl butyral, and the amount of polyvinyl butyral added is 10-12% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material; The dispersant is polyethylene glycol, and the added amount of the polyethylene glycol is 2.8-3.2% of the mass of the raw material powder of the sodium niobate-based lead-free dielectric energy storage ceramic material.
7. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S8, the specific conditions of the isostatic pressing treatment are: temperature 70-80°C, and pressurization pressures of 50MPa, 100MPa, 150MPa and 200MPa respectively.
8. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S9, the debinding treatment is carried out at 550-600°C for 20-24 hours.
9. The method for preparing a high configuration entropy sodium niobate-based lead-free dielectric energy storage ceramic material according to claim 2, characterized in that: In step S10, the sintering conditions are: in a closed condition, the temperature is raised from room temperature to 1100-1300°C at a heating rate of 1.5-3.5°C / min and kept at that temperature for 2-6 hours, and then naturally cooled to room temperature in the furnace.
10. An application of the sodium niobate-based lead-free dielectric energy storage ceramic material as claimed in claim 1, characterized in that: The dielectric energy storage ceramic material is used as an energy storage material in the fields of laser, integrated circuit, electronic information or aerospace.
Citation Information
Patent Citations
Sodium niobate-based ceramic material and preparation method thereof
CN115028450A
High-entropy perovskite oxide doped ceramic, preparation method and application thereof
CN115991599A
Sodium niobate-based lead-free ceramic dielectric material as well as preparation method and application thereof
CN117735984A
High-energy-storage-density sodium niobate-based lead-free ceramic dielectric material and preparation thereof
CN118239774A
Potassium sodium bismuth niobate tantalate zirconate ferrite ceramics with non-stoichiometric nb5+ and preparation method therefor
US20240067572A1