High-temperature heat dissipation ceramic composition for aerospace sandwich panel and preparation method of high-temperature heat dissipation ceramic composition

By using diamond and ceramic compositions of different particle sizes of SiC in aerospace sandwich panels, combining γ-aminopropyltriethoxysilane and photosensitive resin, the problem of low heat dissipation efficiency at high temperatures is solved, and high-efficiency heat The conduction and thermal diffusion properties enhance the stability and reliability of the material.

CN118955143AActive Publication Date: 2024-11-15CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411151811.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-15
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Existing aerospace mezzanine panel materials are prone to cracks and pores at high temperatures, and their heat dissipation efficiency is low, making it impossible to achieve the thermal conductivity of metal composite materials.

Method used

Use diamond and silicon carbide (SiC) mixtures of different particle sizes as ceramic compositions, combined with γ-aminopropyltriethoxysilane and photosensitive resin, and molded by ultrasonic stirring and digital light treatment to form an efficient ceramic slurry, which improves its Thermal conductivity and heat diffusion properties.

Benefits of technology

It significantly improves the thermal conductivity and thermal diffusion coefficient of the aerospace mezzanine panel, effectively prevents cracks and pores caused by high temperatures, enhances the heat dissipation efficiency and reliability of the material, and is close to the performance of metal composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955143A_ABST
    Figure CN118955143A_ABST
Patent Text Reader

Abstract

The invention relates to a ceramic slurry composition and a preparation method thereof, in particular to a high-temperature heat dissipation ceramic composition for aerospace sandwich panels and a preparation method of the high-temperature heat dissipation ceramic composition. The slurry formed by the ceramic composition provided by the invention has excellent heat conduction and heat diffusion, so that the aerospace sandwich panel can effectively prevent cracks and pores caused by ultrahigh temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a ceramic slurry composition and a preparation method thereof, and more particularly to a high-temperature heat dissipation ceramic composition for aerospace sandwich panels and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) ceramics exhibit a range of excellent properties, including high flexural strength, good oxidation and corrosion resistance, excellent wear resistance and high temperature resistance. These properties make SiC the material of choice for thermal protection structures of aerospace vehicles. SiC materials can withstand high heat flux environments at temperatures up to 1000°C without cracking or delamination. This is due to the high thermal conductivity of the SiC matrix at ultra-high temperatures, making SiC composites ideal materials for advanced thermal protection systems of hypersonic aircraft. However, research on laminated manufacturing of solid structures of carbon / carbon materials also focuses on improving the heat transfer performance of the material itself, which is brittle and difficult to process. The volume and weight of the three-dimensional woven sandwich structure SiC composite ceramic sandwich structure increase, thereby reducing the overall heat dissipation efficiency.

[0003] In order to solve the above problems, the use of carbon fiber reinforced SiC lattice sandwich composites to partially or completely replace traditional aircraft materials can significantly reduce the weight of the aircraft while enhancing its high temperature resistance and oxidation resistance (Polymers and Polymer Composites. 2022; 30. doi: 10.1177 / 09673911221098729 ). Additive manufacturing of carbon fiber reinforced SiC ceramic panels combines the technical advantages of efficient heat transfer and heat dissipation, providing thermal conductivity far superior to that of traditional ceramic matrix composites. It also achieves high heat dissipation surface area and lightweight structure, thereby improving the heat dissipation efficiency and reliability of thermally protected ceramic panels. However, mechanical and environmentally induced cracks and pores are almost inevitable at high temperatures; in addition, although the thermal conductivity of carbon fiber reinforced SiC composite ceramics has been improved, it still does not reach the thermal conductivity of metal composites. Summary of the invention

[0004] The purpose of the present invention is to provide a high-temperature heat-dissipating ceramic composition for aerospace sandwich panels to solve the above-mentioned problems existing in the prior art. The slurry formed by the ceramic composition of the present invention should have excellent thermal conductivity and thermal diffusion, so that the aerospace sandwich panels can effectively prevent cracks and pores caused by ultra-high temperatures.

[0005] According to a first aspect of the present invention, the present invention provides a high temperature heat dissipation ceramic composition for aerospace sandwich panels, comprising diamond and SiC.

[0006] Preferably, the SiC is a mixture of 200-500nm SiC and 600-2000nm SiC.

[0007] Preferably, by mass percentage:

[0008]

[0009] The sum of the ingredients in the composition is 100%.

[0010] Preferably, the weight ratio of 200-500 nm SiC to 600-2000 nm SiC is 4:5.

[0011] Preferably, the mass percentage is: 40% of SiC with a size of 200-500 nm, 50% of SiC with a size of 600-2000 nm, 6% of silicon-coated diamond, and 4% of γ-aminopropyltriethoxysilane.

[0012] In the above composition, silicon carbide is a ceramic powder matrix, which enables the slurry to have a shaped frame after sintering; γ-aminopropyltriethoxysilane is used to couple the organic polymer resin and the inorganic ceramic filler; diamond can also promote the improvement of the thermal conductivity and heat dissipation efficiency of the slurry. The combination of these components and the above percentage range of each component are determined through a large number of tests, and the above combination and percentage range enable the coating formed by the coating composition of the present invention to have the above high-efficiency heat dissipation advantage.

[0013] According to a second aspect of the present invention, the present invention provides a method for preparing a high temperature heat dissipation ceramic composition for an aerospace sandwich panel, comprising the following steps:

[0014] (a) drying SiC, preferably drying SiC at 110° C. for 24 hours;

[0015] (b) preparing a mixed solution of anhydrous ethanol and deionized water, preferably preparing a mixed solution of anhydrous ethanol and deionized water in a volume ratio of 1:1.5;

[0016] (c) adding SiC powder to the mixture solution, and then performing ultrasonic stirring to uniformly disperse the SiC powder; preferably, adding SiC powder to the mixture solution, and then performing ultrasonic stirring for 30 minutes to ensure uniform dispersion of the powder.

[0017] (d) γ-aminopropyltriethoxysilane is added to the dispersed solution.

[0018] (e) heating the solution with stirring; preferably, the solution is subjected to magnetic stirring in an oil bath at 50° C. for 4 hours.

[0019] (f) centrifuging the suspension to achieve solid-liquid separation, washing the separated solid, drying, grinding, sieving, and then drying for future use; preferably, centrifuging the suspension to achieve solid-liquid separation, washing the separated solid, drying in a 100° C. hot air drying furnace, grinding, sieving through a 200 mesh sieve, and then drying for future use.

[0020] (g) adding the powder and diamonds in (f) above into a photosensitive resin to form a slurry (such as ANYCUBIC photosensitive resin) and stirring;

[0021] Preferably, the volume fraction of the powder in the ceramic slurry is 45% to 60%.

[0022] Preferably, the optimal mass ratio of 200-500nm SiC to 600-2000nm SiC is 4:5.

[0023] The ceramic composition of the present invention can be formed by conventional digital light processing, and the slurry has excellent high-efficiency heat dissipation after sintering. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Graph showing thermal conductivity and thermal diffusivity of ceramics of the embodiment.

[0025] Figure 2 The microstructure SEM image of the embodiment. DETAILED DESCRIPTION

[0026] In the following examples, the heat transfer characteristics of the structure are represented by thermal conductivity (W / m·k). The higher the value, the faster the heat transfer. The thermal diffusion coefficient (mm 2 / s) represents the heat dissipation characteristics of the structure. The higher the value, the better the heat dissipation.

[0027] Aerospace sandwich panels are composite structures composed of upper and lower thin panels with high strength and a lightweight core material in the middle. The ceramic matrix composite material of the sandwich panel has a series of excellent properties such as high bending strength, good oxidation resistance, good corrosion resistance, good wear resistance and high temperature resistance, making it the preferred material for thermal protection structures of aerospace vehicles. There are two types of sandwich panels: trapezoidal compact structure (TC) sandwich panels and standard hexagonal honeycomb (HC) sandwich panels, with pore sizes between 1 and 4 mm, which are mainly used in nozzles, combustion chambers, turbine stators and other hot sections of aircraft engines such as M882, F100PW229, CFM565B, F135, GEnx, LEAPX, etc.

[0028] Example 1

[0029] At room temperature and pressure, SiC was dried at 110°C for 24 hours according to the mass percentages in Table 1 below, and a mixed solution of an appropriate amount of anhydrous ethanol and deionized water in a volume ratio of 1:1.5 was prepared. SiC powder was added to the mixed solution, and then ultrasonic stirring was performed for 30 minutes to ensure uniform dispersion of the powder, and then γ-aminopropyltriethoxysilane was added. The solution was subjected to magnetic stirring reaction in a 50°C oil bath for 4 hours, and the suspension was centrifuged to achieve solid-liquid separation. The separated solid was washed, dried in a 100°C hot air drying furnace, ground, sieved through a 200-mesh sieve, and then dried for standby use. Then, the silicon-coated diamond powder and SiC powder were mixed with a commercial resin (vertical cubic ANYCUBIC photosensitive resin) according to the mass percentages in Table 1 to form a slurry and stirred for half an hour. The volume fraction of the material powder (i.e., SiC and silicon-coated diamond) in the formed slurry was 46 vol.%.

[0030] The slurry obtained above was 3D printed using a photocuring printing device (ADT-3D-ZP-Printer-Pro-67-35). The sliced ​​model was projected layer by layer onto the slurry composition by a digital light processing projector. After each layer of the projected image was solidified into a thin layer in the area where the resin layer was very thin, the molding table moved one layer and continued to solidify the next layer. This cycle was repeated until the overall printing was completed. After the printing process was completed, the sample was immersed in an ultrasonic cleaner filled with anhydrous ethanol for 2 minutes. The green body was thermally decomposed at 800°C in an argon atmosphere at a heating and cooling rate of 1°C / min for 2 hours. Then, an inorganic porous intermediate composed of decomposed carbon and diamond was obtained by removing organic matter. Subsequently, a reactive melt infiltration process was used to densify the intermediate, in which molten silicon infiltrated into the intermediate, reacted with carbon and diamond, and gradually formed in-situ generated SiC to fill the pores. The reactive melt infiltration process was carried out in a vacuum environment with a vacuum level of 10 - 3 Pa. The temperature was increased at a rate of 10°C / min until it reached 1500°C and then kept at that temperature for 0.5 h. Subsequently, the temperature was decreased to 900°C at a rate of 5°C / min. Finally, the material was cooled to room temperature to prepare a diamond / SiC composite material.

[0031] After sintering, the thermal conductivity and thermal diffusivity of the diamond / SiC composite ceramic material were tested at 400°C to 1000°C. The test results are listed in Table 1.

[0032] Comparative Example 1

[0033] At room temperature and pressure, SiC was dried at 110°C for 24 hours according to the mass percentages in Table 1 below, and a mixed solution of an appropriate amount of anhydrous ethanol and deionized water with a volume ratio of 1:1.5 was prepared. SiC powder was added to the mixed solution, and then ultrasonic stirring was performed for 30 minutes to ensure uniform dispersion of the powder, and then γ-aminopropyltriethoxysilane was added. The solution was subjected to magnetic stirring reaction in a 50°C oil bath for 4 hours, and the suspension was centrifuged to achieve solid-liquid separation. The separated solid was washed, dried in a 100°C hot air drying furnace, ground, sieved through a 200 mesh sieve, and then dried for standby use. Carbon fiber and SiC powder were mixed with commercial resin (vertical cubic ANYCUBIC photosensitive resin) according to the mass percentages in Table 1 to form a slurry and stirred for half an hour. The volume fraction of the material powder (silicon carbide and carbon fiber) in the formed slurry was 46 vol.%. After sintering, the thermal conductivity and thermal diffusivity of the ceramics from 400°C to 1000°C were tested, and the test results are listed in Table 1.

[0034] Comparative Example 2

[0035] At room temperature and pressure, SiC was dried at 110°C for 24 hours according to the mass percentages in Table 1 below, and a mixed solution of an appropriate amount of anhydrous ethanol and deionized water with a volume ratio of 1:1.5 was prepared. SiC powder was added to the mixed solution, and then ultrasonic stirring was performed for 30 minutes to ensure uniform dispersion of the powder, and then γ-aminopropyltriethoxysilane was added. The solution was subjected to magnetic stirring reaction in a 50°C oil bath for 4 hours, and the suspension was centrifuged to achieve solid-liquid separation. The separated solid was washed, dried in a 100°C hot air drying furnace, ground, sieved through a 200 mesh sieve, and then dried for future use. SiC powder was added according to the mass percentages in Table 1 and a commercial resin (vertical cubic ANYCUBIC photosensitive resin) was formed into a slurry and stirred for half an hour. The volume fraction of the material powder in the SiC ceramic slurry was 46vol.%. After sintering, the thermal conductivity and thermal diffusivity of the ceramics from 400°C to 1000°C were tested, and the test results are listed in Table 1.

[0036] The test data of thermal conductivity and thermal diffusion coefficient of sintered ceramic samples of each embodiment and comparative example in Table 1 below show that the ceramic slurry composition of the present invention is obviously superior to the slurry composition of the comparative example in terms of both single performance and comprehensive performance.

[0037] Table 1

[0038]

[0039] Figure 1The results show that with the increase of temperature, the thermal diffusivity of the three materials gradually decreases, especially the thermal diffusivity of SiC at high temperature. Therefore, the thermal conductivity of silicon carbide composites will decrease at high temperatures. Although the thermal conductivity of the material does not change significantly, the thermal diffusivity will decrease. The main reason is that with the increase of the test temperature, the phonon density increases, resulting in intensified collisions, and the mean free path of phonons in the amorphous phase is shorter and significantly reduced, thereby reducing the diffusion coefficient. By reducing the thermal diffusivity at high temperatures, SiC composites can provide better insulation performance, preventing external heat from entering the internal area or transferring internal heat to the external environment. Therefore, reducing the thermal diffusivity can improve the thermal insulation effect and protect the stability of the hypersonic flight system.

[0040] Figure 2 The results show that the diamond / SiC structure has a smooth surface and good structure ( Figure 2 a). The surface of carbon fiber / SiC is relatively smooth, but contains many pits, and the structure formed shows a relatively rough bonding ( Figure 2 b). Compared with the first two materials, the formation of SiC is relatively uneven, and a distinct layered structure is observed ( Figure 2 c) This layered structure is consistent with the forming accuracy of about 50μm, which may lead to weaker bonding strength. The layered structure may be the main reason for the slow heat conduction in the early stage, especially for the Schoen Gyroid structure with a filling rate of 90%.

[0041] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A high temperature heat dissipation ceramic composition for aerospace sandwich panels, comprising diamond and SiC.

2. The high temperature heat dissipating ceramic composition for aerospace sandwich panels according to claim 1, wherein the SiC is a mixture of 200-500nm SiC and 600-2000nm SiC.

3. The high temperature heat dissipation ceramic composition for aerospace sandwich panels according to claim 1, wherein the mass percentage is: The sum of the ingredients in the composition is 100%.

4. The high temperature heat dissipating ceramic composition for aerospace sandwich panels according to claim 1, wherein the weight ratio of SiC of 200-500 nm to SiC of 600-2000 nm is 4:

5.

5. The high-temperature heat dissipating ceramic composition for aerospace sandwich panels according to any one of claims 1 to 4, wherein the mass percentages are: 40% SiC of 200-500nm, 50% SiC of 600-2000nm, 6% silicon-coated diamond, and 4% γ-aminopropyltriethoxysilane.

6. A method for preparing a high temperature heat dissipation ceramic composition for aerospace sandwich panels, comprising the following steps: (a) drying SiC; preferably, drying SiC at 110° C. for 24 hours; (b) preparing a mixed solution of anhydrous ethanol and deionized water; preferably preparing a mixed solution of anhydrous ethanol and deionized water in a volume ratio of 1:1.5; (c) adding SiC powder to the mixture solution, and then performing ultrasonic stirring to uniformly disperse the SiC powder; preferably, adding SiC powder to the mixture solution, and then performing ultrasonic stirring for 30 minutes to ensure uniform dispersion of the powder; (d) adding γ-aminopropyltriethoxysilane to the dispersed solution; (e) heating and stirring the solution; preferably, the solution is subjected to magnetic stirring in an oil bath at 50° C. for 4 hours; (f) centrifuging the suspension to achieve solid-liquid separation, washing the separated solid, drying, grinding, sieving, and then drying for future use; preferably, centrifuging the suspension to achieve solid-liquid separation, washing the separated solid, drying in a hot air drying furnace at 100° C., grinding, sieving through a 200 mesh sieve, and then drying for future use; (g) Add the powder and diamond as described in (f) above into a photosensitive resin to form a slurry and stir.

7. The method according to claim 6, wherein the slurry is shaped by digital light processing and then sintered.

Citation Information

Patent Citations

  • Construction method for directional heat conduction channel of high-thermal-conductivity diamond modified silicon carbide ceramic matrix composite material

    CN109704776A

  • Preparation method of DLP-printed Cf / SiC ceramic green body

    CN113526970A

  • Coreactive three-dimensional printing of parts

    CN113661046A

  • Preparation method of high-thermal-conductivity diamond-silicon carbide multiphase ceramic and heat dissipation substrate

    CN117088690A

  • Ceramic heat dissipation member with improved heat conductivity and emissivity and method for manufacturing same

    KR1020140096637A