Method for enhancing compressive strength of cement mortar by electrifying pre-carbonization method

By applying DC power to cement mortar and passing CO2 into pre-carbonization method, the CO2 emission and mechanical properties problems in silicate cement production are solved, the compressive strength and durability of concrete are improved, and greenhouse gas absorption and cost are realized save.

CN118955171AActive Publication Date: 2024-11-15DALIAN MARITIME UNIVERSITY

Patent Information

Application Number
CN202411043434.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

A large amount of greenhouse gas CO2 is emitted during the production of silicate cement, and carbonization is not good for the mechanical properties of concrete, resulting in corrosion and performance of steel bars.

Method used

The pre-carbonization method is used to apply DC electricity to the cement mortar and continuously pass CO2 into it. It is stirred by a magnetic stirrer to form a pre-carbonized cement slurry and mix it with standard sand and cement mortar to improve the compressive strength of the cement mortar.

Benefits of technology

It significantly improves the mechanical properties and compressive strength of concrete, while absorbing greenhouse gas CO2, reducing costs and extending the service life of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955171A_ABST
    Figure CN118955171A_ABST
Patent Text Reader

Abstract

The method comprises the following steps: mixing 10-15% of total amount of cement and 80% of total amount of mixing water to obtain cement paste, applying direct current to the cement paste for 5-25 minutes, introducing CO2 into the cement paste and continuously stirring to complete pre-carbonization to obtain a pre-carbonized cement paste; pre-carbonized cement paste is obtained; adding the total amount of standard sand, the residual cement in the total amount of cement, the residual mixing water in the total amount of mixing water and the pre-carbonized cement paste into an automatic cement mortar stirrer, and stirring for 3-5 minutes; according to the method, a large amount of greenhouse gas CO2 can be absorbed by introducing CO2 into the cement mortar and applying direct current at the same time, the mechanical property of the concrete is also greatly improved, the CO2 source is very wide, the cost is low, and the mechanical property of the concrete is also greatly improved while the cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a method for strengthening the compressive strength of cement mortar by an electric pre-carbonization method. Background Art

[0002] Concrete with Portland cement as binder is the most widely used building material. The global usage of concrete is second only to water, accounting for 70% of all construction and building materials. Although Portland cement has advantages such as easy use and global availability of raw materials, the production process of Portland cement releases a large amount of greenhouse gas CO2. 1 ton of cement clinker emits 0.98 tons of carbon dioxide equivalent, and the cement industry's carbon dioxide emissions account for 5% of global carbon dioxide emissions.

[0003] The carbon dioxide emitted during the manufacture of Portland cement can be naturally absorbed by concrete products through natural chemical reactions. However, the natural process is too slow and it may take hundreds of years to reabsorb all the emitted carbon dioxide. In addition, carbonation is harmful to concrete and can cause corrosion of steel bars and reduce the mechanical properties of concrete. Summary of the invention

[0004] The present invention provides a method for strengthening the compressive strength of cement mortar by an electric pre-carbonization method to solve the above problems.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] A method for strengthening the compressive strength of cement mortar by an electric pre-carbonization method comprises the following steps:

[0007] S1: Cement mortar includes the total amount of standard sand, the total amount of cement and the total amount of mixing water;

[0008] 10% to 15% of the total amount of cement and 80% of the total amount of mixing water are mixed to obtain cement paste, direct current is applied to the cement paste for 5-25 minutes, and CO2 is introduced into the cement paste while stirring continuously to complete pre-carbonization, thereby obtaining pre-carbonized cement paste;

[0009] S2: Add the total amount of standard sand, the remaining cement in the total amount of cement, the remaining mixing water in the total amount of mixing water, and the pre-carbonized cement slurry into an automatic cement mortar mixer and stir for 3-5 minutes.

[0010] Furthermore, the voltage of the direct current is set to 30V.

[0011] Furthermore, in S1, the method of introducing CO2 is: using an air conditioner to directly blow CO2 into the cement slurry at a gas flow rate of 2 L / min for a time of 5-25 min.

[0012] Furthermore, in S1, in the cement mortar, in parts by weight, the total amount of cement is 525 parts, the total amount of standard sand is 1312.5 parts, and the total amount of mixing water is 262.5 parts.

[0013] Furthermore, in S1, the stirring method is to use a magnetic stirrer for stirring, and the rotation speed of the magnetic stirrer is 900 r / min.

[0014] Furthermore, the purity of the CO2 is 95%-99%.

[0015] Furthermore, the cement is ordinary Portland cement, and its strength grade is 42.5, 42.5R, 52.5 or 52.5R.

[0016] Furthermore, the rotation speed of the automatic cement mortar mixer is 1000-2000rpm.

[0017] The beneficial effects of the present invention are:

[0018] The present invention discloses a method for strengthening the compressive strength of cement mortar by electric pre-carbonization. By introducing CO2 into the cement mortar and applying direct current at the same time, it can not only absorb a large amount of greenhouse gas CO2, but also greatly improve the mechanical properties of concrete. The source of CO2 is also extremely wide and low-cost, which can save costs while greatly improving the mechanical properties of concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 It is a structural schematic diagram of a device used in a method for enhancing the compressive strength of cement mortar by an electrical pre-carbonization method disclosed in an embodiment of the present invention.

[0021] In the figure: 1. DC power supply; 2. Negative steel bar of power supply; 3. Positive carbon rod of power supply; 4. Magnetic stirrer; 5. Air conditioner; 6. Carbon dioxide cylinder; 7. Beaker. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The principles involved in this method are:

[0024] In the process of S1 electrifying and pre-carbonizing cement mortar, carbon dioxide gas first dissolves in water to form carbonic acid, and then carbonic acid dissociates into H + and CO3 2- , H + and CO3 2- Ca released from cement clinker 2+ If more carbon dioxide is added to the cement mortar, some calcium carbonate will dissolve to form calcium bicarbonate, which will dissolve in water (calcium bicarbonate has high solubility in water). Therefore, the carbonized cement mortar will contain rich calcium carbonate particles, Ca 2+ 、HCO3 - and a small amount of CO3 2- The generated calcium carbonate precipitate fills the pores in the cement mortar, reducing the porosity, thereby improving the density and strength of the cement mortar, and improving the compressive strength and durability of the cement mortar; and the application of electricity as a catalytic condition can not only accelerate the reaction rate of the entire process, but also make the water in the cement paste electrolyze to produce more hydrogen ions and hydroxide ions, and can also electrolyze more Ca2+, the key raw material for the formation of calcium carbonate, from the cement paste. 2+ , thereby producing more subsequent products and thus the mechanical properties of concrete;

[0025] After the pre-carbonized cement paste in S2 is mixed with other cement mortar, the Ca(OH)2 produced by cement hydration reacts with HCO3 - Nano- to submicro-CaCO3 particles are generated in situ during the reaction, providing additional heterogeneous nucleation sites for cement hydration, thus greatly improving the hydration performance of cement. On the other hand, adding CO2 to the cement paste through pre-carbonization will change the hydration performance of C3A. The final reaction product is mainly determined by the molar ratio of CO2 / Al2O3 and C3A / SO3. For example, when the molar ratio of C3A / SO3 of cement is close to 1, the hydration reaction formula of C3A modified by CO2 is:

[0026]

[0027] If more CO2 is added, the hemibicarbonate in the above reaction formula is partially or completely replaced by monobicarbonate. From the above reaction formula, it can be seen that adding CO2 to cement mortar will change the mineralogical characteristics of hydrated cement: 1) produce and stabilize more ettringite, 2) produce more monocarbonate, 3) reduce or eliminate monosulfate, all of which are beneficial to the strength and durability of cement mortar. The formation of ettringite produces more solid products. Due to the large volume expansion of ettringite, the porosity of hydrated concrete is reduced, thereby improving the strength of cement mortar.

[0028] Example

[0029] Embodiment 1:

[0030] In a method for strengthening the compressive strength of cement mortar by electric pre-carbonization, step S1 (electric pre-carbonization) is to adopt Figure 1 The device shown in the figure comprises a DC power supply 1, a negative power supply steel bar 2, a positive power supply carbon rod 3, a magnetic stirrer 4, an air conditioner 5, a carbon dioxide gas cylinder 6 and a beaker 7, the positive pole of the DC power supply is electrically connected to the positive power supply carbon rod 3, the negative pole of the DC power supply 1 is electrically connected to the negative power supply steel bar 2, the ends of the positive power supply carbon rod 3 and the negative power supply steel bar 2 are immersed in the cement slurry in the beaker, a magnetic stirrer is provided at the bottom of the beaker, and the CO2 in the carbon dioxide gas cylinder 6 is blown into the cement slurry in the beaker through the air conditioner 5 and the pipeline for power-on pre-carbonization;

[0031] A method for strengthening the compressive strength of cement mortar by electric pre-carbonization method, comprising the steps of:

[0032] S1: Take 15% (78.75 parts by weight) of the total amount of cement and 80% (210 parts by weight) of the total amount of mixing water and add them to a beaker, mix to obtain cement paste, apply 30V direct current to the cement paste for 5 minutes, and use an air conditioner to directly bubble CO2 into the cement paste at a gas flow rate of 2L / min for 5 minutes. The purity of CO2 is 95%. During this process, it is continuously stirred by a magnetic stirrer at a speed of 900r / min. Pre-carbonization is completed to obtain pre-carbonized cement paste; in cement mortar, in terms of weight, the total amount of cement is 525 parts, the total amount of standard sand is 1312.5 parts, and the total amount of mixing water is 262.5 parts; the cement is 42.5 ordinary Portland cement;

[0033] S2: Add the total amount of standard sand, the remaining cement in the total amount of cement, the remaining mixing water in the total amount of mixing water, and the pre-carbonized cement slurry into an automatic cement mortar mixer. The rotation speed of the automatic cement mortar mixer is 2000 rpm, and the mixing time is 3 minutes.

[0034] Embodiment 2:

[0035] The only difference between this embodiment and embodiment 1 is that, in this embodiment, direct current is applied to the cement paste for 10 min, and CO2 is introduced into the cement paste for 10 min.

[0036] Embodiment 3:

[0037] The only difference between this embodiment and embodiment 1 is that, in this embodiment, direct current is applied to the cement paste for 15 minutes, and CO2 is introduced into the cement paste for 15 minutes.

[0038] Embodiment 4:

[0039] The only difference between this embodiment and embodiment 1 is that, in this embodiment, direct current is applied to the cement paste for 20 min, and CO2 is introduced into the cement paste for 20 min.

[0040] Embodiment 5:

[0041] The only difference between this embodiment and embodiment 1 is that, in this embodiment, direct current is applied to the cement paste for 25 minutes, and CO2 is introduced into the cement paste for 25 minutes.

[0042] Comparative Example

[0043] Comparative Example 1

[0044] The difference between this comparative example and Example 1 is that in this comparative example, only CO2 is introduced into the cement paste, and no direct current is applied.

[0045] Comparative Example 2

[0046] The only difference between this comparative example and Example 2 is that in this comparative example, only CO2 is introduced into the cement paste, and no direct current is applied.

[0047] Comparative Example 3

[0048] The difference between this comparative example and Example 3 is that in this comparative example, only CO2 is introduced into the cement paste, and no direct current is applied.

[0049] Comparative Example 4

[0050] The difference between this comparative example and Example 4 is that in this comparative example, only CO2 is introduced into the cement paste, and no direct current is applied.

[0051] Comparative Example 5

[0052] The only difference between this comparative example and Example 5 is that in this comparative example, only CO2 is introduced into the cement paste, and no direct current is applied.

[0053] Comparative Example 6

[0054] The only difference between this comparative example and Example 1 is that in this comparative example, CO2 is not introduced into the cement paste and direct current is not applied.

[0055] The cement mortar composition ratios of Examples 1-5 and Comparative Examples 1-6 and the power-on and CO2-on times are shown in Table 1 below:

[0056] Table 1 Cement mortar mix ratios of Examples 1-5 and Comparative Examples 1-6 and timetables for powering on and CO2 passing on

[0057]

[0058] The compressive strength test was performed on the cement mortars of Examples 1-5 and Comparative Examples 1-6 after being stirred by an automatic cement mortar mixer:

[0059] (1) Methods:

[0060] The cement mortar stirred by the cement mortar automatic mixer was vibrated twice and placed in a triple cube mold with a side length of 70.7 mm. Six test blocks were prepared for each embodiment and each comparative example. After seven days of water bath curing, the average compressive strength of the cement mortar was tested according to the JGJ / T+70-2009+ standard for basic performance test methods of building mortar;

[0061] (2) The results are shown in Table 2

[0062] Table 2 Compressive strength results of Examples 1-5 and Comparative Examples 1-6

[0063]

[0064] It can be seen from the data in Table 2 that the compressive strength of the cement mortars of Examples 1-5 is significantly higher than that of the cement mortars of Comparative Example 6 (no direct current is applied and no CO2 is introduced); moreover, compared with the cement mortars of Comparative Example 1-5 which are only pre-carbonized but not electrified, the compressive strength of the cement mortars of Examples 1-5 which are pre-carbonized and electrified is improved, and under the conditions of Example 2, i.e., when electrification is applied for 10 minutes and CO2 is passed, the compressive strength is improved the most after seven days, which can increase the compressive strength of the cement mortar by 8.59%.

[0065] In summary, by introducing CO2 into cement mortar and applying direct current at the same time, the compressive strength of cement mortar is significantly improved. The method disclosed in the present invention can not only absorb a large amount of greenhouse gas CO2, save costs and promote sustainable development, but also enable cement mortar to withstand greater loads during use, thereby improving the safety and durability of buildings.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for strengthening the compressive strength of cement mortar by electric pre-carbonization, characterized in that: The following steps are involved: S1: Cement mortar includes the total amount of standard sand, the total amount of cement and the total amount of mixing water; 10% to 15% of the total amount of cement and 80% of the total amount of mixing water are mixed to obtain cement paste, direct current is applied to the cement paste for 5-25 minutes, and CO2 is introduced into the cement paste while stirring continuously to complete pre-carbonization, thereby obtaining pre-carbonized cement paste; S2: Add the total amount of standard sand, the remaining cement in the total amount of cement, the remaining mixing water in the total amount of mixing water, and the pre-carbonized cement slurry into an automatic cement mortar mixer and stir for 3-5 minutes.

2. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: The voltage of the direct current is set to 30V.

3. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: In S1, the method of introducing CO2 is: using an air conditioner to directly blow CO2 into the cement paste at a gas flow rate of 2L / min for a period of 5-25min.

4. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: In S1, in the cement mortar, in parts by weight, the total amount of cement is 525 parts, the total amount of standard sand is 1312.5 parts, and the total amount of mixing water is 262.5 parts.

5. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: In S1, the stirring method is to use a magnetic stirrer for stirring, and the rotation speed of the magnetic stirrer is 900r / min.

6. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: The purity of the CO2 is 95%-99%.

7. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: The cement is ordinary Portland cement, and its strength grade is 42.5, 42.5R, 52.5 or 52.5R.

8. The method for strengthening the compressive strength of cement mortar by electric pre-carbonization according to claim 1, characterized in that: The rotation speed of the automatic cement mortar mixer is 1000-2000rpm.

Citation Information

Patent Citations

  • Method for preparing cement and (or) carbonaceous products by converting calcium carbonate based on electrochemical process

    CN115449822A

  • High-viscosity cement paste and preparation method thereof

    CN116283154A

  • Carbonized concrete and preparation method thereof

    CN116477881A

  • Resource utilization method of steel slag and carbon dioxide

    CN118305171A

  • Method for improving quality of reinforced concrete structure

    JP2015074578A

Cited By

  • Method for enhancing performance of cement mortar through acidification electric field pre-carbonization

    CN120349135A

  • Method for enhancing the performance of cement mortar by acidizing electric field pre-carbonization

    CN120349135B