Metal compensation additive and preparation method thereof, metal ion battery positive pole piece, metal ion battery and battery pack

The preparation of metal compensation additives through the acid-base reaction of organic carboxylic acids and alkaline compounds has been solved, and the problems of difficult preparation and poor compatibility in the prior art have been improved, the energy density and cycling performance of metal ion batteries have been improved, and the effective compensation of metal ions has been achieved. And battery performance improvement.

CN118955344APending Publication Date: 2024-11-15SOUTHWEST UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410997088.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing metal compensation additives are difficult to prepare and have poor compatibility with the cathode material, which affects the energy density and cycling performance of metal ion batteries.

Method used

The metal compensation additive is prepared by acid-base reaction of organic carboxylic acids and alkaline compounds, and mixed with the positive electrode active material to form an electrode material with good compatibility.

Benefits of technology

It is achieved to provide additional metal ions during the charging process of the positive electrode active material, compensate for the metal ion loss caused by the formation of the SEI film, improve the energy density and cycling performance of the battery, and do not produce by-products that are harmful to the positive electrode material after decomposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955344A_ABST
    Figure CN118955344A_ABST
Patent Text Reader

Abstract

The invention relates to a metal compensation additive and a preparation method thereof, a metal ion battery positive pole piece, a metal ion battery and a battery pack, and belongs to the technical field of metal battery positive pole material supplements. The metal compensation additive is used in a positive electrode of a lithium ion battery, a positive electrode of a sodium ion battery or a positive electrode of a potassium ion battery, and is prepared by taking organic carboxylic acid and an alkaline compound as raw materials through simple acid-base reaction. An electrochemical performance test shows that the decomposition voltage of the metal compensation additive is lower than the upper limit voltage of a positive electrode material, the metal compensation additive has a feasible metal compensation effect, and a product generated after first-circle decomposition has no influence on a positive electrode active material and also has no influence on the performance after circulation. When the metal compensation additive is used in a metal ion battery or a battery pack, the electrochemical performance of the battery can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal battery positive electrode material supplements, and relates to metal compensation additives and a preparation method thereof, a metal ion battery positive electrode sheet, a metal ion battery and a battery pack. Background Art

[0002] Metal ion batteries (such as sodium / lithium / potassium ion batteries) have abundant raw material reserves, low cost, and high battery safety. They have great application prospects in portable electronic devices and electric vehicles, and are now widely used in energy storage, base stations, electric bicycles, low-end passenger cars and other markets. However, in metal ion batteries, due to the formation of negative electrode SEI, the existence of surface defects and the occurrence of side reactions, active metal ions are consumed, the first effect of metal ion batteries is reduced, and the energy density and cycle performance of the battery are directly affected. Therefore, pre-metallization is needed to solve this problem.

[0003] Premetallization, that is, pre-embedding of metal ions, is considered to be a technology for providing additional sufficient metal sources in electrochemical energy storage systems. According to the technical route, it can be divided into negative electrode compensation and positive electrode compensation. Among them, negative electrode compensation technology was developed earlier, including physical mixing compensation, self-discharge compensation, chemical compensation and electrochemical compensation. Although the negative electrode compensation route can effectively reduce the irreversible capacity loss, it is complicated to operate, has high requirements for the working environment, and is difficult to achieve industrial production. Positive electrode compensation is to mix metal compensation additives with positive electrode materials to form a slurry, and coat it on the current collector to make an electrode to achieve premetallization. In comparison, positive electrode compensation has attracted widespread attention from researchers because of its simple operation, direct adaptation to existing processes and no residual pollution.

[0004] At present, most metal compensating additives are difficult to prepare and have poor compatibility with cathode materials. When used in metal ion batteries, they have high operating voltages or leave byproducts that affect the subsequent cycles of cathode materials after decomposition, which is not conducive to improving the electrochemical performance of the battery. Therefore, it is necessary to develop new metal compensating additives through simple and efficient methods and apply them to batteries. Summary of the invention

[0005] In view of this, one of the objects of the present invention is to provide a metal compensation additive; a second object of the present invention is to provide a method for preparing a metal compensation additive; a third object of the present invention is to provide a metal ion battery positive electrode plate; a fourth object of the present invention is to provide a metal ion battery; and a fifth object of the present invention is to provide a battery pack.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] 1. A metal compensating additive, which is used for any one of a lithium ion battery positive electrode, a sodium ion battery positive electrode or a potassium ion battery positive electrode; the structure of the metal compensating additive is shown in structural formula I, structural formula II or structural formula III:

[0008]

[0009] When the metal compensation additive is used for the positive electrode of a lithium ion battery, wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are independently selected from any one of -H or -CH2COOLi; M is selected from Li;

[0010] When the metal compensation additive is used for the positive electrode of a sodium ion battery, wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are each independently selected from any one of -H or -CH2COONa; M is selected from Na;

[0011] When the metal compensation additive is used for the positive electrode of a potassium ion battery, R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are independently selected from any one of -H or -CH2COOK; and M is selected from K.

[0012] Preferably, when used in a lithium-ion battery cathode, the structure of the metal compensating additive is at least one of the structural formulas (1) to (6):

[0013]

[0014] When used for the positive electrode of a sodium ion battery, the structure of the metal compensation additive is at least one of the structural formulas (7) to (12):

[0015]

[0016] When used for the positive electrode of a potassium ion battery, the structure of the metal compensation additive is at least one of the structural formulas (13) to (18):

[0017]

[0018] 2. The preparation method of the metal compensation additive is as follows:

[0019] The organic carboxylic acid and the alkaline compound are placed in deionized water, and after being fully mixed, a solution is obtained, and then the solution is added dropwise into an organic solvent to obtain a precipitate by a recrystallization method, and the precipitate is dried and ground into a solid powder to obtain a metal compensation additive;

[0020] Alternatively, the organic carboxylic acid and the alkaline compound are placed in deionized water, mixed thoroughly to obtain a solution, and then the water in the solution is evaporated to obtain the metal compensation additive;

[0021] The structure of the organic carboxylic acid is shown in Structural Formula IV, Structural Formula V or Structural Formula VI:

[0022]

[0023] Wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are each independently selected from any one of -H or -CH2COOH;

[0024] When the metal compensation additive is used for the positive electrode of a lithium-ion battery, the alkaline compound is any one of LiOH, Li2CO3 or LiHCO3;

[0025] When the metal compensation additive is used for the positive electrode of a sodium ion battery, the alkaline compound is any one of NaOH, Na2CO3 or NaHCO3;

[0026] When the metal compensation additive is used for the positive electrode of a potassium ion battery: the alkaline compound is any one of KOH, K2CO3 or KHCO3;

[0027] The organic solvent is any one of methanol, ethanol, acetone, ketone and N,N-dimethylformamide.

[0028] Preferably, the molar ratio of the organic carboxylic acid to the basic compound is 1:2-5.

[0029] Preferably, the structure of the organic carboxylic acid is any one of the structural formulas (19) to (24):

[0030]

[0031] 3. A positive electrode plate for a metal ion battery, comprising a positive electrode active material, a conductive agent, a binder and a current collector, and also comprising the metal compensation additive; the mass of the metal compensation additive is 5 to 30% of the total mass of the positive electrode active material, the conductive agent, the binder and the metal compensation additive.

[0032] Preferably, when the metal compensation additive is used for the positive electrode of a lithium-ion battery, the positive electrode active material is any one of lithium iron phosphate, lithium iron manganese phosphate or lithium nickel cobalt manganese oxide;

[0033] When the metal compensation additive is used for the positive electrode of a sodium ion battery, the positive electrode active material is any one of sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium iron phosphate pyrophosphate, sodium nickel manganese titanate or sodium nickel manganese ferrate;

[0034] When the metal compensation additive is used for the positive electrode of a potassium ion battery, the positive electrode active material is any one of potassium vanadium phosphate, potassium vanadium fluorophosphate, potassium iron pyrophosphate, potassium iron sulfate or potassium nickel cobalt manganate;

[0035] The conductive agent is any one or more of carbon nanotubes, acetylene black, Ketjen black, graphene, ordered mesoporous carbon or CMK-3;

[0036] The binder is any one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polytetrafluoroethylene or polyvinyl alcohol;

[0037] The current collector is any one of aluminum foil, carbon-coated aluminum foil or copper foil.

[0038] 4. A metal ion battery, comprising the metal ion battery positive electrode plate.

[0039] 5. A battery pack, comprising a box, a protection plate and the metal ion battery; the metal ion battery and the protection plate are arranged in the box; the metal ion batteries are connected in series, in parallel or in a combination of series and parallel.

[0040] The beneficial effects of the present invention are as follows: 1. The present invention provides a metal compensating additive and a preparation method thereof, wherein the metal compensating additive is used in a positive electrode of a lithium ion battery, a positive electrode of a sodium ion battery or a positive electrode of a potassium ion battery. The metal compensating additive is mainly prepared by an acid-base reaction of an organic carboxylic acid and an alkaline compound, and the preparation method is simple and easy to operate.

[0041] 2. The present invention also provides a metal ion battery positive electrode sheet, a metal ion battery and a battery pack. The metal ion battery positive electrode sheet, the metal ion battery and the battery pack all contain the above-mentioned metal compensation additive. The experimental results show that the prepared metal compensation additive can provide additional metal ions during the charging process of the positive electrode active material, which is used to make up for the metal ions lost due to the formation of the SEI film during the first cycle of charging and discharging of the positive electrode active material, and has good compatibility with the positive electrode material. The byproducts left by the decomposition will not cause adverse reactions in long cycles, which is beneficial to improve the energy density and cycle performance of the metal ion battery or battery pack.

[0042] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0044] Figure 1 The SEM image and EDS image of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1, wherein (a) is the SEM image and (b) is the EDS image;

[0045] Figure 2 The SEM image and EDS image of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 2, wherein (a) is the SEM image and (b) is the EDS image;

[0046] Figure 3 The SEM image and EDS image of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 3, wherein (a) is the SEM image and (b) is the EDS image;

[0047] Figure 4 The specific capacity-voltage curve diagram of a button cell when the positive electrode sheet constructed based on the sodium supplement additive obtained in Example 1 is assembled;

[0048] Figure 5 The specific capacity-voltage curve diagram of a button cell when the positive electrode sheet constructed based on the sodium supplement additive obtained in Example 2 is assembled;

[0049] Figure 6 The specific capacity-voltage curve diagram of a button cell when the positive electrode sheet constructed based on the sodium supplement additive obtained in Example 3 is assembled;

[0050] Figure 7 The specific capacity-voltage curve diagram of a button cell when the positive electrode sheet constructed based on the lithium supplement additive obtained in Example 7 is assembled;

[0051] Figure 8 The specific capacity-voltage curve diagram of a button cell when the positive electrode sheet constructed based on the potassium supplement additive obtained in Example 8 is assembled;

[0052] Fig. 9 The voltage-specific capacity curves corresponding to the first cycle of the half-cell assembled based on the positive electrode sheet of the sodium ion battery prepared in Example 10 and the half-cell assembled based on the positive electrode sheet of the sodium ion battery without the sodium supplement prepared in Comparative Example 1;

[0053] Fig.10 The voltage-specific capacity curves corresponding to the first cycle of the half-cell assembled based on the positive electrode sheet of the sodium ion battery prepared in Example 13 and the half-cell assembled based on the positive electrode sheet of the sodium ion battery without the sodium supplement agent prepared in Comparative Example 2;

[0054] Fig.11The figure is a structural diagram of a battery pack prepared based on the metal ion battery of the present invention. DETAILED DESCRIPTION

[0055] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.

[0056] Example 1

[0057] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0058] 0.1 mol 2,2'-thiodiacetic acid The mixture was placed in deionized water with 0.2 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0059] Figure 1 (a) shows that the metal compensating additive for the positive electrode of the sodium ion battery prepared in Example 1 is in the form of a flake, with a size of about 5 to 10 μm; Figure 1 (b) shows that the metal compensating additive contains S element, thereby proving that the metal compensating additive is successfully synthesized.

[0060] Example 2

[0061] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0062] 0.1 mol 3,3'-thiodipropionic acid The mixture was placed in deionized water with 0.2 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0063] Figure 2(a) shows that the morphology of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 2 is agglomerated small particles with a size of about 1 to 2 μm; Figure 2 (b) shows that the metal compensating additive contains S element, thereby proving that the metal compensating additive is successfully synthesized.

[0064] Example 3

[0065] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0066] 0.1 mol 2,2'-thiodisuccinic acid The mixture was placed in deionized water with 0.4 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0067] Figure 3 (a) shows that the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 3 is in the form of particles with a size of about 100 to 300 nm; Figure 3 (b) shows that the metal compensating additive contains S element, thereby proving that the metal compensating additive is successfully synthesized.

[0068] Example 4

[0069] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0070] 0.1 mol of 2,2'-sulfinyldiacetic acid The mixture was placed in deionized water with 0.2 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0071] Example 5

[0072] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0073] 0.1 mol carboxymethylsulfonylacetic acid The mixture was placed in deionized water with 0.2 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0074] Example 6

[0075] A metal compensating additive for a sodium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0076] 0.1 mol 2-carboxymethylsulfosuccinic acid The product was placed in deionized water with 0.3 mol NaOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0077] Example 7

[0078] A metal compensating additive for a lithium ion battery positive electrode, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0079] 0.1 mol 2,2'-thiodiacetic acid The mixture was placed in deionized water with 0.2 mol LiOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0080] Example 8

[0081] A metal compensating additive for a positive electrode of a potassium ion battery, the structural formula of the metal compensating additive is The specific preparation method is as follows:

[0082] 0.1 mol 2,2'-thiodiacetic acid The product was placed in deionized water with 0.2 mol KOH and stirred for 0.5 h to obtain a solution. The solution was then added dropwise into ethanol to obtain a precipitate by recrystallization. The precipitate was then dried by suction filtration and finally ground into a solid powder.

[0083] Similarly, a scanning electron microscope was used to observe the morphology of the metal compensation additives prepared in Examples 4 to 8, and an EDS spectrometer was used to detect the distribution of S in each metal compensation additive. The experimental results showed that the S element could be detected in each metal compensation additive, indicating that the method of the present invention can successfully synthesize lithium compensation additives, sodium compensation additives and potassium compensation additives.

[0084] Example 9

[0085] Preparation of positive electrode sheet for sodium ion battery 1

[0086] By weight, 75 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring, and then the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 1.

[0087] Example 10

[0088] Preparation of positive electrode for sodium ion battery 2

[0089] By weight, 70 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring, and then the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 2.

[0090] Embodiment 11

[0091] Preparation of positive electrode for sodium ion battery 3

[0092] By weight, 65 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 15 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring, and then the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 3.

[0093] Example 12

[0094] Preparation of positive electrode for sodium ion battery

[0095] By weight, 75 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 4.

[0096] Embodiment 13

[0097] Preparation of positive electrode for sodium ion battery 5

[0098] By weight, 70 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 5.

[0099] Embodiment 14

[0100] Preparation of positive electrode for sodium ion battery 6

[0101] By weight, 65 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 15 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 1 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300 μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 6.

[0102] Embodiment 15

[0103] Preparation of positive electrode for sodium ion battery

[0104] By weight, 70 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 2 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300 μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 7.

[0105] Example 16

[0106] Preparation of positive electrode for sodium ion battery

[0107] By weight, 70 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 3 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 8.

[0108] Embodiment 17

[0109] Preparation of positive electrode sheet for sodium ion battery

[0110] By weight, 70 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 4 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 9.

[0111] Embodiment 18

[0112] Preparation of positive electrode sheet for sodium ion battery 10

[0113] By weight, 70 parts of positive electrode active material (Na2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 5 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 10.

[0114] Embodiment 19

[0115] Preparation of positive electrode for sodium ion battery 11

[0116] By weight, 70 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the sodium ion battery prepared in Example 6 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 11.

[0117] Embodiment 20

[0118] Preparation of positive electrode sheet for lithium-ion battery 12

[0119] By weight, 70 parts of positive electrode active material (LiFePO4), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the lithium ion battery prepared in Example 7 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the lithium ion battery positive electrode sheet 12.

[0120] Embodiment 21

[0121] Preparation of positive electrode for potassium ion battery 13

[0122] By weight, 70 parts of positive electrode active material (K3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 10 parts of the metal compensation additive for the positive electrode of the potassium ion battery prepared in Example 8 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the potassium ion battery positive electrode sheet 13.

[0123] Embodiment 22

[0124] Preparation of positive electrode sheet for sodium ion battery 14

[0125] By weight, 70 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 1 and 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 2 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 14.

[0126] Embodiment 23

[0127] Preparation of positive electrode for sodium ion battery 15

[0128] By weight, 70 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 1 and 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 3 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 15.

[0129] Embodiment 24

[0130] Preparation of positive electrode for sodium ion battery 16

[0131] By weight, 70 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 2 and 5 parts of metal compensation additives for the positive electrode of the sodium ion battery prepared in Example 3 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 16.

[0132] Embodiment 25

[0133] Preparation of positive electrode for sodium ion battery 17

[0134] By weight, 70 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then 5 parts of metal compensation additive for the positive electrode of sodium ion battery prepared in Example 1, 5 parts of metal compensation additive for the positive electrode of sodium ion battery prepared in Example 2, and 5 parts of metal compensation additive for the positive electrode of sodium ion battery prepared in Example 3 are added, and then NMP solvent is added, and a uniform slurry is obtained by stirring. Then, the slurry is evenly coated on the carbon-coated aluminum foil with a 300μm scraper, and the carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain the sodium ion battery positive electrode sheet 17.

[0135] Comparative Example 1

[0136] Preparation of sodium ion battery positive electrode sheet without sodium supplementation agent 18

[0137] By weight, 80 parts of positive electrode active material (Na 2 / 3 Ni 1 / 3 Mn 1 / 3 Ti 1 / 3 O2), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF), and then add NMP solvent, and stir to obtain a uniform slurry. Then use a 300μm scraper to evenly coat the slurry on the carbon-coated aluminum foil, and then dry and slice the carbon-coated aluminum foil coated with the slurry in turn to obtain a sodium ion battery positive electrode sheet 18 without a sodium supplement.

[0138] Comparative Example 2

[0139] Preparation of sodium ion battery positive electrode sheet without sodium supplementation agent19

[0140] By weight, 80 parts of positive electrode active material (Na3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then NMP solvent is added. A uniform slurry is obtained by stirring, and then the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper. The carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain a sodium ion battery positive electrode sheet 19 that does not contain a sodium supplement.

[0141] Comparative Example 3

[0142] Preparation of positive electrode sheet of lithium-ion battery without lithium supplementation agent

[0143] By weight, 80 parts of positive electrode active material (LiFePO4), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then NMP solvent is added and stirred to obtain a uniform slurry. Then, a 300μm scraper is used to evenly coat the slurry on the carbon-coated aluminum foil. The carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain a lithium-ion battery positive electrode sheet 20 without a lithium supplement.

[0144] Comparative Example 4

[0145] Preparation of positive electrode sheet of potassium ion battery without potassium supplement

[0146] By weight, 80 parts of positive electrode active material (K3V2(PO4)2F3), 10 parts of conductive agent (acetylene black), and 10 parts of binder (PVDF) are mixed, and then NMP solvent is added. A uniform slurry is obtained by stirring, and then the slurry is evenly coated on the carbon-coated aluminum foil using a 300μm scraper. The carbon-coated aluminum foil coated with the slurry is dried and sliced ​​in turn to obtain a potassium ion battery positive electrode sheet 21 without a potassium supplement.

[0147] The positive electrode sheets obtained in Examples 9 to 25 and Comparative Examples 1 to 4 were placed in a glove box filled with argon gas to assemble button cells to obtain half-cells. The button cell model was CR2032, the negative electrodes were metal sodium sheets, lithium sheets or potassium sheets, the separator was glass fiber, and the electrolyte was 1 mol / L NaClO4 in EC-DEC-FEC. Each half-cell was placed in a voltage range of 2.5 to 4.5 V and the electrochemical performance was tested at a current density of 30 mA / g. The test results are shown in Table 1.

[0148] Table 1 Electrochemical properties of button cells prepared based on the positive electrode sheets in Examples 9 to 25 and Comparative Examples 1 to 4

[0149]

[0150]

[0151] Table 1 compares the actual capacity retention rate of the button cells prepared based on the positive electrode sheets in Examples 9 to 25 and Comparative Examples 1 to 4 after long cycles. It can be seen that the products generated by the prepared metal compensation additives after the first cycle decomposition will not affect the positive electrode active material, nor will they affect the performance after the cycle, indicating that no products with side effects on the positive electrode cycle are left after decomposition. The positive electrode sheet constructed based on the sodium supplement additive obtained in Example 1 is assembled into a button cell (such as Figure 4 As shown), the positive electrode sheet constructed based on the sodium supplement additive obtained in Example 2 is assembled into a button battery (as shown Figure 5 As shown), the positive electrode sheet constructed based on the sodium supplement additive obtained in Example 3 is assembled into a button battery (as shown Figure 6 As shown), the positive electrode sheet constructed based on the lithium supplement additive obtained in Example 7 is assembled into a button battery (as shown Figure 7 As shown) and the positive electrode sheet constructed based on the potassium supplement additive obtained in Example 8 are assembled into a button battery (as shown Figure 8 From the specific capacity-voltage curve diagram (as shown in the figure), it can be seen that the decomposition voltages of the metal compensation additives in the positive electrode sheets of these five metal ion batteries are all between 3.8 and 4.3 V, and can provide a specific capacity higher than 350 mAh / g, and the decomposition voltage is lower than the upper limit voltage of the positive electrode active material, proving that the metal compensation additives in the present invention have a feasible metal compensation effect.

[0152] Compare the half-cell assembled based on the positive electrode sheet of the sodium ion battery prepared in Example 10 and the half-cell assembled based on the positive electrode sheet of the sodium ion battery without the sodium supplement prepared in Comparative Example 1 (such as Fig. 9 As shown) and a half-cell assembled based on the positive electrode sheet of the sodium ion battery prepared in Example 13 and a half-cell assembled based on the positive electrode sheet of the sodium ion battery without sodium supplement prepared in Comparative Example 2 (as shown Fig.10The voltage-specific capacity corresponding to the first cycle (as shown) can be used to illustrate that the metal compensation additive for the positive electrode of the sodium ion battery is suitable for layered oxides and polyanion positive electrodes, proving the universality of the metal compensation additive. In addition, by comparing Examples 9 to 11 and Examples 12 to 14, it can be found that the addition amount of the metal compensation additive for the positive electrode of the sodium ion battery will not cause side reactions between 5% and 15%. As the addition amount of the metal compensation additive for the positive electrode of the sodium ion battery increases, the first cycle charging specific capacity of the half-cell will increase accordingly, indicating that the effect of sodium compensation is very obvious, and the addition amount can be selected according to actual needs. By comparing Example 13 with Examples 22 to 25, it is found that when more than one sodium supplement additive is used, the sodium supplement effect of the first cycle can be further increased. This may be due to the synergistic effect between the sodium supplement additives, and the sodium compensation effect on the positive electrode active material is more obvious. At the same time, the cycle retention rate is also improved, which further proves that the products produced by the decomposition of the sodium supplement additive in the present invention will not have a negative impact on the battery. Similarly, by exploring the experimental effects of metal compensation additives for lithium-ion battery positive electrodes and metal compensation additives for potassium-ion battery positive electrodes, similar conclusions can be drawn as to metal compensation additives for sodium-ion battery positive electrodes, indicating that the metal compensation additives prepared by the present invention are extremely suitable for metal compensation in lithium, sodium, and potassium ion batteries.

[0153] The metal ion battery constructed with the above metal (Li / Na / K) compensating additive can be used in a battery pack. Fig.11 As shown, the battery pack is composed of multiple metal ion batteries, a protection board and a box. Among them, each metal ion battery and the protection board are arranged in the box, and each metal ion battery can be connected in series, in parallel, or in a combination of series and parallel, so that the battery pack has a higher capacity and a higher voltage, so that it can be suitable for various application scenarios. The protection board can prevent the metal ion battery from overcharging, over-discharging, overcurrent, short circuit and ultra-high temperature charging and discharging, and stop the operation in time, ensuring the safety of the battery pack.

[0154] In summary, the present invention provides a metal compensation additive and a preparation method thereof, a metal ion battery positive electrode plate, a metal ion battery and a battery pack. The metal compensation additive is used for the positive electrode of a lithium ion battery, a sodium ion battery positive electrode or a potassium ion battery positive electrode, and is prepared by a simple acid-base reaction. Electrochemical performance tests show that the metal compensation additive has a feasible metal compensation effect, and the products generated after the first cycle of decomposition will not affect the positive electrode active material, nor will they affect the performance after the cycle. After decomposition, no products with side effects on the positive electrode cycle are left, and its application in metal ion batteries or battery packs is beneficial to improving the electrochemical performance of the battery.

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A metal compensating additive, characterized in that: The metal compensation additive is used for any one of the positive electrodes of lithium ion batteries, sodium ion batteries or potassium ion batteries; the structure of the metal compensation additive is shown in structural formula I, structural formula II or structural formula III: When the metal compensation additive is used for the positive electrode of a lithium ion battery, wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are independently selected from any one of -H or -CH2COOLi; M is selected from Li; When the metal compensation additive is used for the positive electrode of a sodium ion battery, wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are each independently selected from any one of -H or -CH2COONa; M is selected from Na; When the metal compensation additive is used for the positive electrode of a potassium ion battery, R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are independently selected from any one of -H or -CH2COOK; and M is selected from K.

2. The metal compensating additive according to claim 1, characterized in that: When used for the positive electrode of a lithium-ion battery, the structure of the metal compensation additive is at least one of the structural formulas (1) to (6): When used for the positive electrode of a sodium ion battery, the structure of the metal compensation additive is at least one of the structural formulas (7) to (12): When used for the positive electrode of a potassium ion battery, the structure of the metal compensation additive is at least one of the structural formulas (13) to (18):

3. The method for preparing the metal compensating additive according to any one of claims 1 or 2, characterized in that: The preparation method is as follows: The organic carboxylic acid and the alkaline compound are placed in deionized water, and after being fully mixed, a solution is obtained, and then the solution is added dropwise into an organic solvent to obtain a precipitate by a recrystallization method, and the precipitate is dried and ground into a solid powder to obtain a metal compensation additive; Alternatively, the organic carboxylic acid and the alkaline compound are placed in deionized water, mixed thoroughly to obtain a solution, and then the water in the solution is evaporated to obtain the metal compensation additive; The structure of the organic carboxylic acid is shown in Structural Formula IV, Structural Formula V or Structural Formula VI: Wherein R1 and R2 are simultaneously selected from any one of -CH or -CHCH2; R3 and R4 are each independently selected from any one of -H or -CH2COOH; When the metal compensation additive is used for the positive electrode of a lithium-ion battery, the alkaline compound is any one of LiOH, Li2CO3 or LiHCO3; When the metal compensation additive is used for the positive electrode of a sodium ion battery, the alkaline compound is any one of NaOH, Na2CO3 or NaHCO3; When the metal compensation additive is used for the positive electrode of a potassium ion battery: the alkaline compound is any one of KOH, K2CO3 or KHCO3; The organic solvent is any one of methanol, ethanol, acetone, ketone and N,N-dimethylformamide.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the organic carboxylic acid to the basic compound is 1:2-5.

5. The preparation method according to claim 3, characterized in that: The structure of the organic carboxylic acid is any one of structural formulas (19) to (24):

6. A positive electrode sheet for a metal ion battery, comprising a positive electrode active material, a conductive agent, a binder and a current collector, characterized in that: It also contains the metal compensation additive according to any one of claims 1 or 2; the mass of the metal compensation additive is 5 to 30% of the total mass of the positive electrode active material, the conductive agent, the binder and the metal compensation additive.

7. The positive electrode plate of a metal ion battery according to claim 6, characterized in that: When the metal compensation additive is used for the positive electrode of a lithium-ion battery, the positive electrode active material is any one of lithium iron phosphate, lithium iron manganese phosphate or lithium nickel cobalt manganese oxide; When the metal compensation additive is used for the positive electrode of a sodium ion battery, the positive electrode active material is any one of sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium iron phosphate pyrophosphate, sodium nickel manganese titanate or sodium nickel manganese ferrate; When the metal compensation additive is used for the positive electrode of a potassium ion battery, the positive electrode active material is any one of potassium vanadium phosphate, potassium vanadium fluorophosphate, potassium iron pyrophosphate, potassium iron sulfate or potassium nickel cobalt manganate; The conductive agent is any one or more of carbon nanotubes, acetylene black, Ketjen black, graphene, ordered mesoporous carbon or CMK-3; The binder is any one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, polytetrafluoroethylene or polyvinyl alcohol; The current collector is any one of aluminum foil, carbon-coated aluminum foil or copper foil.

8. A metal ion battery, characterized in that: The metal ion battery comprises the metal ion battery positive electrode sheet according to any one of claims 6 or 7.

9. A battery pack, characterized in that: The battery pack is composed of a box, a protection plate and the metal ion battery according to claim 8; the metal ion battery and the protection plate are arranged in the box; the metal ion batteries are connected in series, parallel or a combination of series and parallel.

Citation Information

Cited By

  • Potassium ion battery, positive plate or negative plate and preparation method thereof

    CN119560642A