Rosin-based epoxy Vitrimer with fluorescent property as well as preparation method and application of rosin-based epoxy Vitrimer
The rosin-based epoxy Vitrimer material prepared under solvent-free and catalyst-free conditions solves the problem that traditional thermoset polymer materials are difficult to recycle and reuse, and realizes controllable recycling and low environmental impact of thermoset materials, with excellent mechanics and fluorescence Performance, suitable for a variety of applications.
Patent Information
- Application Number
- CN202411030285.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Traditional thermoset polymer materials are difficult to recycle due to their irreversible three-dimensional permanent network structure, and a large number of petroleum-based products and solvents are used during the preparation process, resulting in waste of resources and environmental pollution.
Using solvent-free and catalyst-free conditions, the renewable biomass resource rosin and epoxy resin are reacted through epoxy protonic acid ring-opening to prepare a rosin-based epoxy Vitrimer material with self-healing, reprocessing and chemical degradation properties. .
Controllable recycling of thermosetting materials under mild conditions is achieved, the dependence on non-renewable petroleum resources is reduced, environmental pollution is reduced, and the material has excellent mechanical properties and fluorescent properties, and is suitable for adhesives and information transmission applications.
Smart Images

Figure CN118955867A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a rosin-based epoxy Vitrimer with fluorescent properties, a preparation method and application thereof, and belongs to the technical field of chemical materials. Background Art
[0002] Traditional polymer materials can be divided into thermosetting polymer materials and thermoplastic polymer materials. Thermoplastic polymers have the characteristics of being heated, melted, and hardened after cooling, so they generally have the advantage of being reusable, but their mechanical properties and thermal stability are generally poor, which greatly limits the application of the material. Thermosetting resins are widely used in various industries due to their excellent mechanical properties and solvent resistance. However, due to the irreversible three-dimensional permanent network structure in thermosetting resins after curing, they lose their reprocessing performance, resulting in a waste of resources. In addition, thermosetting resins and their curing agents are mostly petroleum-based products, and long-term use causes environmental pollution problems. Using bio-based resources to gradually replace petroleum-based resources, introducing reversible dynamic covalent bonds, and preparing bio-based "Vitrimer" resins that have the reprocessability of thermoplastic materials and the excellent mechanical properties of thermosetting materials can largely solve the above problems.
[0003] Currently, the raw materials used to prepare epoxy Vitrimer are mostly petrochemical-based products, which are not in line with the concept of sustainable development, and a large amount of solvents and catalysts are required in the preparation process. Summary of the invention
[0004] The purpose of the present invention is to provide a rosin-based epoxy Vitrimer with fluorescent properties, a preparation method thereof and an application thereof. In the present invention, the rosin-based epoxy resin obtained by the ring-opening reaction of rosin, a renewable biomass resource, and epoxy resin through epoxy proton acid is subjected to a further ring-opening reaction with a dibasic acid to obtain a rosin-based epoxy Vitrimer material with self-healing, reprocessing and chemical degradation properties, thereby solving the problem that traditional thermosetting polymer materials are difficult to recycle and reuse, and realizing the controllable recycling of thermosetting materials under mild conditions.
[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:
[0006] A rosin-based epoxy Vitrimer with fluorescent properties, the structural formula of which is as follows:
[0007]
[0008] Among them, n=0, 0.2, 0.4, 0.5, 2.3, 4.7; the wavy lines indicate the omission of repeating units.
[0009] The preparation method of the rosin-based epoxy Vitrimer with fluorescent properties comprises the following steps: firstly reacting hydrogenated acrylic rosin (HAR) with bisphenol A epoxy resin (EP n ) was acidic ring-opened under the catalysis of triphenylphosphine to obtain rosin-based epoxy resin (HAR-EP n ), and then rosin-based epoxy resin (HAR-EP n ) and malic acid (MA) under solvent-free and catalyst-free conditions to obtain HAR-EP n -MA x No solvent is required during the entire reaction process.
[0010] The rosin-based epoxy Vitrimer with fluorescent properties is referred to as HAR-EP n -MA x , x = carboxyl content / epoxy content.
[0011] Rosin-based epoxy resin (HAR-EP n ) is:
[0012]
[0013] Among them, n=0, 0.2, 0.4, 0.5, 2.3, 4.7.
[0014] The bisphenol A type epoxy resin is at least one of bisphenol A diglycidyl ether, E-51 epoxy resin, E-44 epoxy resin, E-42 epoxy resin, E-20 epoxy resin or E-12 epoxy resin.
[0015] In order to further take into account the comprehensive performance of the rosin-based epoxy Vitrimer, preferably, the bisphenol A type epoxy resin is E-51 epoxy resin.
[0016] In order to take into account both product performance and yield, the mass ratio of hydrogenated acrylic rosin to bisphenol A epoxy resin is 1: (1.5-8); malic acid (MA) to rosin-based epoxy resin (HAR-EP n ) is 1:(8-15);
[0017] As a specific implementation scheme, the preparation method of the above-mentioned rosin-based epoxy Vitrimer with fluorescent properties comprises the following steps:
[0018] 1) Stir hydrogenated acrylic rosin, bisphenol A epoxy resin and triphenylphosphine at a temperature of 130-160°C until the acid value is less than 1 mgKOH / g to obtain HAR-EP n; Wherein, the molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol A epoxy resin is 1:(2-2.1); triphenylphosphine is used as a catalyst, and the mass amount of triphenylphosphine is 1-3g / 500g total mass, and the total mass is the sum of the mass of hydrogenated acrylic rosin and bisphenol A epoxy resin;
[0019] 2) Add malic acid (MA) to HAR-EP at a temperature of 120-135°C n After stirring and reacting in the melt, a rosin-based epoxy Vitrimer prepolymer is obtained, which is poured into a mold while hot and cured at high temperature to obtain HAE-EP n -MA x Among them, HAR-EP n The molar ratio of the epoxy group in the malic acid (MA) to -COOH is 1:(0.6-1.0), preferably 1:1.
[0020] In the above step 1), the carboxyl group in the rosin structure is an active modification site. With epoxy resin as a raw material, an acidic ring-opening reaction with rosin can be carried out under the conditions of solvent-free, triphenylphosphine catalysis, and temperature of 130-160° C. to obtain a rosin-based epoxy resin. The molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol A type epoxy resin is more preferably 1:2, so that the grafting rate of hydrogenated acrylic rosin on the rosin-based epoxy resin is higher, and the ring-opening reaction is easier to proceed.
[0021] In the above step 2), the material used for the mold can be selected from polytetrafluoroethylene, silicone or glass. Preferably, the material used for the mold is polytetrafluoroethylene, so that the rosin-based epoxy Vitrimer material is easy to demold after complete curing.
[0022] To ensure complete curing, a step-by-step curing method is adopted. In step 2), high-temperature curing is sequentially curing at 120-130°C for 1-2h, curing at 140-150°C for 1-2h and curing at 160-170°C for 1-2h; the stirring speed of step 1) is 100-300rpm; the reaction time is 1-2h; the heating rate of step 2) is 2-4°C / min, the stirring speed is 100-300rpm, and the reaction time is 10-30min.
[0023] The rosin-based epoxy Vitrimer with fluorescent properties in the present application can be recycled and reused, and can also be completely degraded. Recycling method: grind the recycled rosin-based epoxy Vitrimer into powder, and hot press it in a hot press at 170-180°C and 8-10MPa for 20-30 minutes to obtain the rosin-based epoxy Vitrimer again; Degradation method: grind the recycled rosin-based epoxy Vitrimer into powder, place it in anhydrous ethanol, and act in a pressure reactor at a temperature of 170-180°C and a pressure of 2-3Mpa for 6-8 hours, so that the powder is completely dissolved in the anhydrous ethanol, and the degradation is completed, and the degradation liquid can be used to obtain the rosin-based epoxy Vitrimer material again.
[0024] During the above degradation, 15 to 25 mL of anhydrous ethanol is used for every 1 g of rosin-based epoxy Vitrimer.
[0025] The above-mentioned rosin-based epoxy Vitrimer with fluorescent properties can be used as an adhesive.
[0026] One specific implementation scheme for use as an adhesive is to place the rosin-based epoxy Vitrimer prepolymer between two substrates at a temperature of 65-95°C and a pressure of 15-25N / m 2 The two substrates are stably bonded together by treating them under hot pressing conditions for 1 to 3 minutes and curing them at high temperature; wherein the high temperature curing is sequentially curing at 120 to 130° C. for 1 to 2 hours, curing at 140 to 150° C. for 1 to 2 hours, and curing at 160 to 170° C. for 1 to 2 hours.
[0027] The above-mentioned rosin-based epoxy Vitrimer material with fluorescent properties can also be used in fluorescent anti-counterfeiting and / or information transmission, and emits cyan light of about 500nm under the excitation of ultraviolet light.
[0028] When applied to information transmission, it can be used to make brackets, correctors, deformation mechanisms, controllers or sensors, etc.
[0029] The technologies not mentioned in the present invention are all referred to the prior art.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention uses renewable biomass resources rosin and malic acid as raw materials. The rosin undergoes a ring-opening reaction with epoxy resin in the absence of solvent to obtain a rosin-based epoxy resin. The rosin-based epoxy resin then undergoes a ring-opening reaction with malic acid in the absence of catalyst and solvent to obtain a Vitrimer material. The preparation process is green and environmentally friendly, the raw materials used are inexpensive, and the preparation cost is low. At the same time, the dependence on non-renewable petroleum resources can be reduced, and the recycling of thermosetting materials can be achieved.
[0032] (2) The rosin-based epoxy Vitrimer material prepared by the present invention contains a dynamically reversible β-hydroxy ester bond and has the characteristics of thermal stimulation and alcohol degradation, so that the Vitrimer exhibits self-healing, reprocessing, and physical and chemical recycling capabilities, broadening the research field of Vitrimer.
[0033] (3) The rosin-based epoxy Vitrimer material prepared by the present invention can be used in adhesives, and the bonding strength of stainless steel can reach 24Mpa, which is higher than that of traditional epoxy resins.
[0034] (4) The rosin-based epoxy Vitrimer material prepared by the present invention has a strong fluorescent property. Under the excitation of ultraviolet light, it can emit cyan light of about 500nm, and the quantum yield can reach 10.78%. It can be used for fluorescent anti-counterfeiting, which broadens the application value of rosin and realizes the high-value sustainable utilization of rosin.
[0035] (5) The rosin-based epoxy Vitrimer material prepared by the invention has triple shape memory properties based on Tg and Tv, a high glass transition temperature, and good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 For HAR-EP 0.2 -MA x Tensile strength;
[0037] Figure 2 For HAR-EP 0.2 -MA x Lap shear strength when bonding stainless steel;
[0038] Figure 3 HAREP under different heating time 0.2 -MA x The healing status of
[0039] Figure 4 It is the triple shape memory of HAR-EP0.2-MA1.0. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with the embodiments. The examples are only for explanation and are not intended to limit the present invention in any way. Unless otherwise specified, the raw materials and reagents used in the examples are conventional products that can be obtained commercially; the experimental methods in the examples where specific conditions are not specified are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer.
[0041] In each example, if no temperature is specified, the reaction was carried out at room temperature (15-25° C.); the stirring speed was 200 r / min.
[0042] Example 1
[0043] Hydrogenated acrylic rosin (Shenzhen Guiteng Industrial Co., Ltd.) and E-51 epoxy resin (Shanghai MacLean Biochemical Technology Co., Ltd.) were mixed in a molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol E-51 epoxy resin of 1:2, and stirred at 150°C for acidic ring-opening reaction under triphenylphosphine catalysis. The mass amount of triphenylphosphine was 1g / 500g total mass. A 0.1mol / L KOH standard solution was used to accurately monitor the reaction progress every half an hour. The reaction was stopped when the acid value of the mixed system was less than 1mgKOH / g. The reaction took 1.5 hours and was cooled. The disappearance of epoxy peak and carboxyl peak and the appearance of ester characteristic peak were observed by Fourier transform infrared spectrometer (FT-IR). The structure was further characterized by nuclear magnetic resonance, indicating that the rosin-based epoxy resin HAR-EP 0.2 Successfully synthesized.
[0044] The prepared rosin-based epoxy resin HAR-EP 0.2 The mixture was melted at 130°C, and then malic acid was added. After stirring at 130°C for 20 minutes, a uniformly mixed rosin-based epoxy Vitrimer prepolymer was obtained. The mixture was poured into a polytetrafluoroethylene mold while hot, and cured at 130°C for 2 hours, 150°C for 2 hours, and 170°C for 2 hours. The mixture was naturally cooled to room temperature to obtain a rosin-based epoxy Vitrimer material, which was recorded as HAR-EP. 0.2 -MA 1.0 ; The molar ratio of the epoxy group in the rosin-based epoxy resin to the carboxyl group in the malic acid is 1:1.0; the heating rate during curing is 3°C / min.
[0045] After testing, the glass transition temperature of rosin-based epoxy Vitrimer material is 102°C.
[0046] The stress-strain curve of rosin-based epoxy Vitrimer material is as follows: Figure 1 As shown by Figure 1 It can be seen that due to the rigid skeleton of rosin, the material exhibits excellent mechanical properties and shows a stress of 28.2 MPa, which can meet the basic mechanical property requirements.
[0047] Adhesion performance test: The adhesion performance of rosin-based epoxy Vitrimer materials was measured by a microcomputer-controlled electronic tensile testing machine at a tensile speed of 5 mm min. -1Each type of sample was tested 5 times. The uniformly mixed rosin-based epoxy Vitrimer prepolymer was evenly placed between two identical stainless steel substrates (100mm×25mm×1.6mm), the coverage area of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 25mm×12.5mm, the thickness of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 0.2mm, and the temperature was 65℃ and the pressure was 15N / m 2 The two ends of the two substrates were fixed together with paper clips and cured at 130℃ for 2h, 150℃ for 2h and 170℃ for 2h. The measured bonding strength was as follows: Figure 2 As shown, it can reach 24.8MPa.
[0048] Self-healing experiment: After scratching the rosin-based epoxy Vitrimer material with a blade (the scratch width is 225μm and the depth is 0.2mm), a glass slide is placed on the surface and placed on a hot plate at 130℃. The scratch on the surface of the material gradually heals within 0 to 15 minutes. Figure 3 As shown, the healing rate is 46.7%, indicating that the prepared rosin-based epoxy Vitrimer material has efficient self-healing properties.
[0049] Shape memory experiment: changing the shape of the spline, such as Figure 4 As shown, HAR-EP 0.2 -MA 1.0 At 120°C (above Tg), it bends into an "S" shape and cools to 25°C to obtain an "S" shape. When the temperature is reheated to 120°C, the temporary "S" shape recovers to a permanent rectangle, indicating that HAR-EP 0.2 -MA 1.0 The glass has a shape memory property based on Tg. In addition, to demonstrate that HAR-EP 0.2 -MA 1.0 Triple shape memory of glass, HAR-EP 0.2 -MA 1.0 It was bent into an “O” shape at 180°C, stored for 30 min for topological freezing transformation, and a permanent “O” shape was obtained after cooling to 25°C. 0.2 -MA 1.0 Deformed into a spiral shape at 120°C, cooled to 25°C. When reheated to 100°C, the spiral shape returns to a permanent "O" shape, and only when heated to 180°C does DTER occur, HAR-EP 0.2 -MA 1.0 to restore to a rectangular shape. This shows that HAR-EP 0.2 -MA 1.0 The glass body has triple shape memory.
[0050] Recycling experiment: (a) Physical recycling: The rosin-based epoxy Vitrimer material was ground into powder with a particle size of less than 100 μm, and hot-pressed in a hot press at 180°C and 10 MPa for 30 minutes. The rosin-based epoxy Vitrimer material was molded into a complete sample again. The mechanical property recovery rate of the sample after recycling can reach 64%, indicating that the prepared rosin-based epoxy Vitrimer material has reprocessability; (b) Chemical recycling: 1 g of rosin-based epoxy Vitrimer material powder with a particle size of less than 100 μm was placed in 20 mL of anhydrous ethanol, and degraded in a pressure reactor at 180°C and 3 MPa for 8 hours. After that, all the solids dissolved in the solution, indicating that the prepared rosin-based epoxy Vitrimer material can be chemically degraded, and the degradation liquid can be used to solidify again to obtain the rosin-based epoxy Vitrimer material.
[0051] Fluorescence performance: The fluorescence performance of HAR-EP-MA was tested using a fluorescence spectrometer. Under 390nm ultraviolet light excitation, HAR-EP 0.2 -MA 1.0 It emits fluorescence at around 500nm.
[0052] Example 2
[0053] Hydrogenated acrylic rosin (Shenzhen Guiteng Industrial Co., Ltd.) and E-51 epoxy resin (Shanghai MacLean Biochemical Technology Co., Ltd.) were mixed in a molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol E-51 epoxy resin of 1:2, and stirred at 150°C under triphenylphosphine catalysis for acidic ring-opening reaction. The mass amount of triphenylphosphine was 1g / 500g total mass. A 0.1mol / L KOH standard solution was used to accurately monitor the reaction progress every half an hour. The reaction was stopped when the acid value of the mixed system was less than 1mgKOH / g. The reaction took 1.5h and was cooled. The disappearance of epoxy peak and carboxyl peak and the appearance of ester characteristic peak were observed by Fourier transform infrared spectrometer (FT-IR). The structure was further characterized by nuclear magnetic resonance, indicating that the rosin-based epoxy resin HAR-EP 0.2 Successfully synthesized.
[0054] The prepared rosin-based epoxy resin HAR-EP 0.2 The mixture was melted at 130°C, and then malic acid was added. After stirring at 130°C for 20 minutes, a uniformly mixed rosin-based epoxy Vitrimer prepolymer was obtained. The mixture was poured into a polytetrafluoroethylene mold while hot, and cured at 130°C for 2 hours, 150°C for 2 hours, and 170°C for 2 hours. The mixture was naturally cooled to room temperature to obtain a rosin-based epoxy Vitrimer material, which was recorded as HAR-EP. 0.2 -MA 0.8; The molar ratio of the epoxy group in the rosin-based epoxy resin to the carboxyl group in the malic acid is 1:0.8; the heating rate during curing is 3°C / min.
[0055] According to the test, the glass transition temperature of rosin-based epoxy Vitrimer material is 100°C.
[0056] The stress-strain curve of rosin-based epoxy Vitrimer material is as follows: Figure 1 As shown by Figure 1 It can be seen that due to the rigid skeleton of rosin, the material exhibits excellent mechanical properties and shows a stress of 22.7 MPa, which can meet the basic mechanical property requirements.
[0057] Adhesion performance test: The adhesion performance of rosin-based epoxy Vitrimer materials was measured by a microcomputer-controlled electronic tensile testing machine at a tensile speed of 5 mm min. -1 Each type of sample was tested 5 times. The uniformly mixed rosin-based epoxy Vitrimer prepolymer was evenly placed between two identical stainless steel substrates (100mm×25mm×1.6mm), the coverage area of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 25mm×12.5mm, the thickness of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 0.2mm, and the temperature was 65℃ and the pressure was 15N / m 2 The two ends of the two substrates were fixed together with paper clips and cured at 130℃ for 2h, 150℃ for 2h and 170℃ for 2h. The measured bonding strength was as follows: Figure 2 As shown, it can reach 20.8MPa.
[0058] Self-healing experiment: After scratching the rosin-based epoxy Vitrimer material with a blade (the scratch width is 240μm and the depth is 0.2mm), a glass slide is placed on the surface and placed on a hot plate at 130℃. The scratch on the surface of the material gradually heals within 0 to 15 minutes. Figure 3 As shown, the healing rate is 43.8%, indicating that the prepared rosin-based epoxy Vitrimer material has efficient self-healing properties.
[0059] Shape memory experiment: changing the shape of a spline, HAR-EP 0.2 -MA 0.8 At 120°C (above Tg), it bends into an "S" shape and cools to 25°C to obtain an "S" shape. When the temperature is reheated to 120°C, the temporary "S" shape recovers to a permanent rectangle, indicating that HAR-EP 0.2 -MA 0.8 The glass has a shape memory property based on Tg. In addition, to demonstrate that HAR-EP 0.2 -MA0.8 Triple shape memory of glass, HAR-EP 0.2 -MA 0.8 It was bent into an “O” shape at 180°C, stored for 30 min for topological freezing transformation, and a permanent “O” shape was obtained after cooling to 25°C. 0.2 -MA 0.8 Deformed into a spiral shape at 120°C, cooled to 25°C. When reheated to 100°C, the spiral shape returns to a permanent "O" shape, and only when heated to 180°C does DTER occur, HAR-EP 0.2 -MA 0.8 to restore to a rectangular shape. This shows that HAR-EP 0.2 -MA 0.8 The glass body has triple shape memory.
[0060] Recycling experiment: (a) Physical recycling: The rosin-based epoxy Vitrimer material was ground into powder with a particle size of less than 100 μm, and hot-pressed in a hot press at 180°C and 10 MPa for 30 minutes. The rosin-based epoxy Vitrimer material was molded into a complete sample again. The mechanical property recovery rate of the sample after recycling can reach 58%, indicating that the prepared rosin-based epoxy Vitrimer material has reprocessability; (b) Chemical recycling: 1 g of rosin-based epoxy Vitrimer material powder with a particle size of less than 100 μm was placed in 20 mL of anhydrous ethanol, and degraded in a pressure reactor at 180°C and 3 MPa for 8 hours. After that, all the solids dissolved in the solution, indicating that the prepared rosin-based epoxy Vitrimer material can be chemically degraded, and the degradation liquid can be used to solidify again to obtain the rosin-based epoxy Vitrimer material.
[0061] Fluorescence performance: The fluorescence performance of HAR-EP-MA was tested using a fluorescence spectrometer. Under 390nm ultraviolet light excitation, HAR-EP 0.2 -MA 1.0 It can emit fluorescence at around 500nm.
[0062] Example 3
[0063] Hydrogenated acrylic rosin (Shenzhen Guiteng Industrial Co., Ltd.) and E-51 epoxy resin (Shanghai MacLean Biochemical Technology Co., Ltd.) were mixed in a molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol E-51 epoxy resin of 1:2, and stirred at 150°C under triphenylphosphine catalysis for acidic ring-opening reaction. The mass amount of triphenylphosphine was 1g / 500g total mass. A 0.1mol / L KOH standard solution was used to accurately monitor the reaction progress every half an hour. The reaction was stopped when the acid value of the mixed system was less than 1mgKOH / g. The reaction took 1.5h and was cooled. The disappearance of epoxy peak and carboxyl peak and the appearance of ester characteristic peak were observed by Fourier transform infrared spectrometer (FT-IR). The structure was further characterized by nuclear magnetic resonance, indicating that the rosin-based epoxy resin HAR-EP 0.2 Successfully synthesized.
[0064] The prepared rosin-based epoxy resin HAR-EP 0.2 The mixture was melted at 130°C, and then malic acid was added. After stirring at 130°C for 20 minutes, a uniformly mixed rosin-based epoxy Vitrimer prepolymer was obtained. The mixture was poured into a polytetrafluoroethylene mold while hot, and cured at 130°C for 2 hours, 150°C for 2 hours, and 170°C for 2 hours. The mixture was naturally cooled to room temperature to obtain a rosin-based epoxy Vitrimer material, which was recorded as HAR-EP. 0.2 -MA 0.6 ; The molar ratio of the epoxy group in the rosin-based epoxy resin to the carboxyl group in the malic acid is 1:0.6; the heating rate during curing is 3°C / min.
[0065] After testing, the glass transition temperature of the rosin-based epoxy Vitrimer material is 95°C.
[0066] The stress-strain curve of rosin-based epoxy Vitrimer material is as follows: Figure 1 As shown by Figure 1 It can be seen that due to the rigid skeleton of rosin, the material exhibits excellent mechanical properties and shows a stress of 21.4 MPa, which can meet the basic mechanical property requirements.
[0067] Adhesion performance test: The adhesion performance of rosin-based epoxy Vitrimer materials was measured by a microcomputer-controlled electronic tensile testing machine at a tensile speed of 5 mm min. -1Each type of sample was tested 5 times. The uniformly mixed rosin-based epoxy Vitrimer prepolymer was evenly placed between two identical stainless steel substrates (100mm×25mm×1.6mm), the coverage area of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 25mm×12.5mm, the thickness of the uniformly mixed rosin-based epoxy Vitrimer prepolymer was 0.2mm, and the temperature was 65℃ and the pressure was 15N / m 2 The two ends of the two substrates were fixed together with paper clips and cured at 130℃ for 2h, 150℃ for 2h and 170℃ for 2h. The measured bonding strength was as follows: Figure 2 As shown, it can reach 14.2MPa.
[0068] Self-healing experiment: After scratching the rosin-based epoxy Vitrimer material with a blade (the scratch width is 175μm and the depth is 0.2mm), a glass slide is placed on the surface and placed on a hot plate at 130℃. The scratch on the surface of the material gradually heals within 0 to 15 minutes. Figure 3 As shown, the healing rate is 31.4%, indicating that the prepared rosin-based epoxy Vitrimer material has efficient self-healing properties.
[0069] Shape memory experiment: changing the shape of a spline, HAR-EP 0.2 -MA 0.8 At 120°C (above Tg), it bends into an "S" shape and cools to 25°C to obtain an "S" shape. When the temperature is reheated to 120°C, the temporary "S" shape recovers to a permanent rectangle, indicating that HAR-EP 0.2 -MA 0.8 The glass has a shape memory property based on Tg. In addition, to demonstrate that HAR-EP 0.2 -MA 0.8 Triple shape memory of glass, HAR-EP 0.2 -MA 0.8 It was bent into an “O” shape at 180°C, stored for 30 min for topological freezing transformation, and a permanent “O” shape was obtained after cooling to 25°C. 0.2 -MA 0.8 Deformed into a spiral shape at 120°C, cooled to 25°C. When reheated to 100°C, the spiral shape returns to a permanent "O" shape, and only when heated to 180°C does DTER occur, HAR-EP 0.2 -MA 0.8 to restore to a rectangular shape. This shows that HAR-EP 0.2 -MA 0.8 The glass has three shape memories.
[0070] Recycling experiment: (a) Physical recycling: The rosin-based epoxy Vitrimer material was ground into powder with a particle size of less than 100 μm, and hot-pressed in a hot press at 180°C and 10 MPa for 30 min. The rosin-based epoxy Vitrimer material was molded into a complete sample again. The mechanical property recovery rate of the sample after recycling can reach 50%, indicating that the prepared rosin-based epoxy Vitrimer material has reprocessability; (b) Chemical recycling: 1 g of rosin-based epoxy Vitrimer material powder with a particle size of less than 100 μm was placed in 20 mL of anhydrous ethanol, and degraded in a pressure reactor at 180°C and 3 MPa for 8 hours. After that, all the solids dissolved in the solution, indicating that the prepared rosin-based epoxy Vitrimer material can be chemically degraded, and the degradation liquid can be used to solidify again to obtain the rosin-based epoxy Vitrimer material.
[0071] Fluorescence performance: The fluorescence performance of HAR-EP-MA was tested using a fluorescence spectrometer. Under 390nm ultraviolet light excitation, HAR-EP 0.2 -MA 1.0 It can emit fluorescence at around 500nm.
Claims
1. A rosin-based epoxy Vitrimer with fluorescent properties, characterized in that: Its structural formula is as follows: Among them, n=0, 0.2, 0.4, 0.5, 2.3, 4.
7.
2. The method for preparing the rosin-based epoxy Vitrimer having fluorescent properties according to claim 1, characterized in that: Rosin-based epoxy Vitrimer with fluorescent properties is prepared by ring-opening of rosin-based epoxy resin and malic acid in the absence of solvent and catalyst; wherein the rosin-based epoxy resin is prepared by ring-opening of hydrogenated acrylic rosin and bisphenol A epoxy resin in the absence of solvent.
3. The preparation method according to claim 2, characterized in that: The bisphenol A type epoxy resin is at least one of bisphenol A diglycidyl ether, E-51 epoxy resin, E-44 epoxy resin, E-42 epoxy resin, E-20 epoxy resin or E-12 epoxy resin.
4. The preparation method according to claim 2 or 3, characterized in that: The bisphenol A type epoxy resin adopts E-51 epoxy resin.
5. The preparation method according to claim 2 or 3, characterized in that: The following steps are involved: 1) stirring hydrogenated acrylic rosin, bisphenol A epoxy resin and triphenylphosphine at a temperature of 130-160° C. to react until the acid value is less than 1 mgKOH / g, to obtain a rosin-based epoxy resin; wherein the molar ratio of -COOH in hydrogenated acrylic rosin to epoxy group in bisphenol A epoxy resin is 1:(2-2.1); the mass amount of triphenylphosphine is 1-3 g / 500 g total mass; wherein the total mass is the sum of the masses of hydrogenated acrylic rosin and bisphenol A epoxy resin; 2) Adding malic acid to a rosin-based epoxy resin melt at a temperature of 120-135° C., stirring for reaction, obtaining a rosin-based epoxy vitrimer prepolymer, pouring the prepolymer into a mold while hot, and curing at high temperature to obtain a rosin-based epoxy vitrimer with fluorescent properties; wherein the molar ratio of the epoxy group in the rosin-based epoxy resin to the -COOH in the malic acid is 1:(0.6-1.0).
6. The preparation method according to claim 5, characterized in that: In step 2), the high temperature curing is sequentially curing at 120-130°C for 1-2h, curing at 140-150°C for 1-2h and curing at 160-170°C for 1-2h; the stirring speed of step 1) is 100-300rpm; the reaction time is 1-2h; the heating rate of step 2) is about 2-4°C / min, the stirring speed is 100-300rpm, and the reaction time is 10-30min.
7. A method for reprocessing the rosin-based epoxy Vitrimer with fluorescent properties as claimed in claim 1, characterized in that: The invention comprises recycling and degradation. The recycling method comprises grinding the recovered rosin-based epoxy Vitrimer into powder, hot pressing the powder for 20 to 30 minutes at 170 to 180° C. and 8 to 10 MPa in a hot press, and obtaining the rosin-based epoxy Vitrimer again. The degradation method comprises grinding the recovered rosin-based epoxy Vitrimer into powder, placing the powder in anhydrous ethanol, and reacting the powder in a pressure reactor at a temperature of 170 to 180° C. and a pressure of 2 to 3 MPa for 6 to 8 hours, wherein the powder is completely dissolved in the anhydrous ethanol, and degradation is completed. The degradation liquid can be used to obtain the rosin-based epoxy Vitrimer material again.
8. The use of the rosin-based epoxy Vitrimer with fluorescent properties as claimed in claim 1, characterized in that: Used as adhesive.
9. The use according to claim 8, characterized in that: Place the rosin-based epoxy Vitrimer prepolymer between two substrates at a temperature of 65-95°C and a pressure of 15-25 N / m 2 The two substrates are stably bonded together by treating them under hot pressing conditions for 1 to 3 minutes and curing them at high temperature; wherein the high temperature curing is sequentially curing at 120 to 130° C. for 1 to 2 hours, curing at 140 to 150° C. for 1 to 2 hours, and curing at 160 to 170° C. for 1 to 2 hours.
10. The use of the rosin-based epoxy Vitrimer material with fluorescent properties as claimed in claim 1, characterized in that: It is used in fluorescent anti-counterfeiting and / or information transmission, and emits blue light of about 500nm under the excitation of ultraviolet light.
Citation Information
Patent Citations
Rosin-based vitrimer, preparation method thereof and application of rosin-based vitrimer in preparation of carbon fiber composite material
CN114835880A
Full-rosinyl epoxy glass polymer material as well as preparation method and application thereof
CN115028842A
Rosin-based epoxy resin with fluorescent property as well as preparation method and application thereof
CN116606422A
Daidzein-based epoxy resin material and preparation method thereof
CN116948147A
Dynamic crosslinking recoverable elastomer and preparation method thereof
CN117757169A