TiMn-MOF luminescent material and preparation method thereof

By preparing TiMn-MOF luminescent materials, the harm of rare earth metal organic frames to the environment and the lack of non-rare earth metal red light emission materials are solved, and the effect of efficient red light emission under ultraviolet light is achieved, providing an environmentally friendly solution .

CN118955929AActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411038613.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing rare earth metal organic frame luminescent materials are harmful to the environment and lack materials that non-rare earth metal organic frames can emit red light.

Method used

Using the preparation method of TiMn-MOF luminescent material, tetraMn-MOF luminescent material is used to stir the tetrabutyl titanate and tricarboxylic acid tetrahydrate in a mixed solvent of ethanol, water and dimethyl diamide, and tetrabutyl titanate is added, and then stirred and baked after ultrasonic stirring. Dry, and prepare a TiMn-MOF material that is capable of excitating and emitting 700 nm red light at a wavelength of 350 nm.

Benefits of technology

It realizes a TiMn-MOF luminescent material with simple preparation process and good thermal stability, which can emit red light under ultraviolet light, providing an environmentally friendly red light emission solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955929A_ABST
    Figure CN118955929A_ABST
Patent Text Reader

Abstract

The invention discloses a TiMn-MOF luminescent material and a preparation method thereof, and belongs to the technical field of luminescent materials. The preparation method comprises the following steps: dissolving manganese chloride tetrahydrate and trimesic acid in a mixed solvent composed of ethanol, water and dimethyl diamide, and stirring to obtain a mixed solution A; adding tetrabutyl titanate into the mixed solution A, uniformly stirring, then ultrasonically stirring, centrifugally separating, cleaning with ethanol, and drying to obtain the TiMn-MOF. The TiMn-MOF luminescent material disclosed by the invention is prepared by a stirring method, the preparation process is simple, and the prepared TiMn-MOF luminescent material can be excited under light of 350nm to emit red light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to a TiMn-MOF luminescent material and a preparation method thereof. Background Art

[0002] As a new type of porous crystalline material constructed by metal cations / clusters and organic ligands, luminescent metal-organic frameworks (MOFs) have clear high porosity, chemical and structural tunability, and different luminescent properties, and have great potential in the field of luminescence. Metal-organic frameworks with different morphologies can be synthesized by selecting different metal ions and organic ligands for reaction. The metal ions used to synthesize luminescent metal-organic frameworks (MOFs) are generally rare earth ions. In addition, luminescent MOF materials have significant advantages. The framework material has a rigid and repetitive porous structure that allows the organic luminophores to be arranged in an orderly manner at appropriate spacings, which increases the solid loading of the organic luminophores and is conducive to the excitation of the internal luminophores.

[0003] In recent years, rare earth metal organic framework luminescent materials have attracted more and more attention from the society. Patent application CN106832311A discloses that Eu-MOF multicolor luminescent crystal material and Tb-MOF green light crystal material not only have good thermal stability and light stability, but also have high luminescence efficiency, and are excellent new high-efficiency luminescent crystal materials. Patent application CN116925381A discloses a MOF material with a copper-lanthanum bimetallic structure. The bimetallic MOF material exhibits a fluorescence emission peak at 700nm under the excitation of 405nm blue light. Patent application CN115322389A synthesized a dual-emission europium-based AIE-MOF for the first time, which has both the emission wavelength of europium and the AIE emission wavelength of tetraphenylethylene tetracarboxylic acid, and has good application prospects. However, since rare earth metal organic frameworks can cause harm to the environment, the present invention needs to explore a non-rare earth metal organic framework luminescent material that can emit red light. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a TiMn-MOF luminescent material and a preparation method thereof.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0007] (1) dissolving manganese chloride tetrahydrate and trimesic acid in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirring to obtain a mixed solution A;

[0008] (2) adding tetrabutyl titanate to the mixed solution A and stirring evenly to obtain a mixed solution B;

[0009] (3) The mixed solution B is ultrasonically stirred, then centrifuged and washed with ethanol, and then dried to obtain TiMn-MOF.

[0010] As a preferred embodiment of the present invention, the volume ratio of ethanol, water and dimethyl diamide is 1:1:(1-2).

[0011] As a preferred embodiment of the present invention, the mass ratio of manganese chloride tetrahydrate to trimesic acid is 3-13:6-10.

[0012] As a preferred embodiment of the present invention, the concentration of manganese chloride tetrahydrate in the mixed solution A is 3-13 g / L, and the concentration of trimesic acid is 6-10 g / L.

[0013] As a preferred embodiment of the present invention, the volume ratio of the solution A to tetrabutyl titanate is (61-63):(1-3).

[0014] As a preferred embodiment of the present invention, in the step (3), the ultrasonication time is not less than 10 minutes, and the stirring time is 3-8 hours.

[0015] The present invention also claims to protect the TiMn-MOF luminescent material prepared by the preparation method of the TiMn-MOF luminescent material.

[0016] As a preferred embodiment of the present invention, the excitation wavelength of the TiMn-MOF luminescent material is 350 nm, and the emission wavelength is 700 nm.

[0017] The luminescence principle of the material of the present invention:

[0018] After being excited by a 350nm wavelength, the TiMn-MOF material goes through three stages: absorption, energy transfer, and light emission. After the light is absorbed, the electrons jump from a low energy level to a high energy level, and then emit photons when they jump back to a lower energy level or the ground state energy level, generating visible light.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The TiMn-MOF luminescent material of the present invention is prepared by a stirring method, the preparation process is simple, and the prepared TiMn-MOF luminescent material can be excited under 350nm light, and generates 700nm red light through three stages of absorption, energy transfer and light emission. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the X-ray diffraction pattern of TiMn-MOF prepared in Example 1.

[0022] Figure 2 These are scanning electron microscope images of the TiMn-MOF prepared in Example 1 and their elemental analysis images, wherein (a) is a scanning electron microscope image of the TiMn-MOF at low magnification, (b) is a scanning electron microscope image of the TiMn-MOF at high magnification, C is a mapping distribution map of the C element, O is a mapping distribution map of the O element, Ti is a mapping distribution map of the Ti element, and Mn is a mapping distribution map of the Mn element.

[0023] Figure 3 This is the thermogravimetric diagram of the TiMn-MOF prepared in Example 1.

[0024] Figure 4 This is the excitation and emission spectra of TiMn-MOF prepared in Example 1. DETAILED DESCRIPTION

[0025] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0026] Example 1

[0027] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0028] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of manganese chloride tetrahydrate added to the mixed solvent is 3.8 g / L, and the amount of trimesic acid added is 7 g / L.

[0029] (2) Tetrabutyl titanate was added to 61 mL of mixed solution A and stirred for 10 min to obtain mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 1.2 mL.

[0030] (3) The mixed solution B was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0031] from Figure 1 It can be concluded that TiMn-MOF contains TiO2 and Mn2O3 components, and no impurity peaks appear.

[0032] from Figure 2 It can be seen that the structure of TiMn-MOF is uniform and spherical, the particles are about 800nm, its surface presents a mesh texture, and the C, O, Ti, and Mn elements are evenly distributed, and the Mn content is relatively low.

[0033] like Figure 3 As shown in Figure 2, TiMn-MOF has good thermal stability, so it has application value in a wide range. Figure 4 It can be seen that the TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0034] Example 2

[0035] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0036] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of manganese chloride tetrahydrate added to the mixed solvent is 4.2 g / L, and the amount of trimesic acid added is 8 g / L.

[0037] (2) Tetrabutyl titanate was added to 63 mL of mixed solution A, and the mixture was stirred for 10 min to obtain a mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 1.6 mL.

[0038] (3) The mixed solution B was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0039] When the TiMn-MOF material prepared in this embodiment is irradiated with a 4W handheld ultraviolet lamp, it can be observed that the TiMn-MOF material emits red light. The TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0040] Example 3

[0041] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0042] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of manganese chloride tetrahydrate added to the mixed solvent is 4.8 g / L, and the amount of trimesic acid added is 9 g / L.

[0043] (2) Tetrabutyl titanate was added to 62 mL of mixed solution A, and the mixture was stirred for 10 min to obtain a mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 2.1 mL.

[0044] (3) The mixed solution B was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0045] When the TiMn-MOF material prepared in this embodiment is irradiated with a 4W handheld ultraviolet lamp, it can be observed that the TiMn-MOF material emits red light. The TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0046] Example 4

[0047] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0048] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of manganese chloride tetrahydrate added to the mixed solvent is 6 g / L, and the amount of trimesic acid added is 9.2 g / L.

[0049] (2) Tetrabutyl titanate was added to 61 mL of mixed solution A, and the mixture was stirred for 10 min to obtain a mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 2.4 mL.

[0050] (3) The mixed solution B was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0051] When the TiMn-MOF material prepared in this embodiment is irradiated with a 4W handheld ultraviolet lamp, it can be observed that the TiMn-MOF material emits red light. The TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0052] Example 5

[0053] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0054] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:2, the amount of manganese chloride tetrahydrate added to the mixed solvent is 13 g / L, and the amount of trimesic acid added is 10 g / L.

[0055] (2) Tetrabutyl titanate was added to 62 mL of mixed solution A, and the mixture was stirred for 10 min to obtain a mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 3 mL.

[0056] (3) The mixed solution B was ultrasonically treated for 6 min, stirred for 8 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0057] When the TiMn-MOF material prepared in this embodiment is irradiated with a 4W handheld ultraviolet lamp, it can be observed that the TiMn-MOF material emits red light. The TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0058] Example 6

[0059] A method for preparing a TiMn-MOF luminescent material comprises the following steps:

[0060] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:2, the amount of manganese chloride tetrahydrate added to the mixed solvent is 3 g / L, and the amount of trimesic acid added is 6 g / L.

[0061] (2) Tetrabutyl titanate was added to 61 mL of mixed solution A and stirred for 10 min to obtain mixed solution B, wherein the amount of tetrabutyl titanate in solution B was 1 mL.

[0062] (3) The mixed solution B was ultrasonically treated for 5 min, stirred for 3 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain TiMn-MOF.

[0063] When the TiMn-MOF material prepared in this embodiment is irradiated with a 4W handheld ultraviolet lamp, it can be observed that the TiMn-MOF material emits red light. The TiMn-MOF material prepared in this embodiment can be excited by 350nm light and emit 700nm red light, so the material emits red light under ultraviolet light.

[0064] Comparative Example 1

[0065] A method for preparing a Mn-MOF luminescent material comprises the following steps:

[0066] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of manganese chloride tetrahydrate added to the mixed solvent is 3.8 g / L, and the amount of trimesic acid added is 7 g / L.

[0067] (2) The mixed solution A was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain Mn-MOF.

[0068] The Mn-MOF prepared in Comparative Example 1 was excited by 350nm light and emitted reddish-brown light.

[0069] Comparative Example 2

[0070] A method for preparing a Ti-MOF luminescent material comprises the following steps:

[0071] (1) Manganese chloride tetrahydrate and trimesic acid are dissolved in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirred to obtain a mixed solution A; wherein the volume ratio of ethanol, deionized water and dimethyl diamide is 1:1:1, the amount of tetrabutyl titanate added to the mixed solvent is 1.2 mL, and the amount of trimesic acid added is 7 g / L.

[0072] (2) The mixed solution A was ultrasonically treated for 10 min, stirred for 3.5 h, then centrifuged and washed with ethanol three times, and dried in a drying oven at 60 °C for 12 h to obtain Ti-MOF.

[0073] The Ti-MOF material prepared in Comparative Example 2 cannot be excited by 350nm light.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a TiMn-MOF luminescent material, characterized in that: The steps include: (1) dissolving manganese chloride tetrahydrate and trimesic acid in a mixed solvent consisting of ethanol, water and dimethyl diamide and stirring to obtain a mixed solution A; (2) adding tetrabutyl titanate to the mixed solution A and stirring evenly to obtain a mixed solution B; (3) The mixed solution B is ultrasonically stirred, then centrifuged and washed with ethanol, and then dried to obtain TiMn-MOF.

2. The method for preparing the TiMn-MOF luminescent material according to claim 1, characterized in that: The volume ratio of the ethanol, water and dimethyl diamide is 1:1:(1-2).

3. The method for preparing the TiMn-MOF luminescent material according to claim 1, characterized in that: The concentration of manganese chloride tetrahydrate in the mixed solution A is 3-13 g / L, and the concentration of trimesic acid is 6-10 g / L.

4. The method for preparing the TiMn-MOF luminescent material according to claim 1, characterized in that: The volume ratio of the solution A to tetrabutyl titanate is (61-63):(1-3).

5. The method for preparing the TiMn-MOF luminescent material according to claim 1, characterized in that: In the step (3), the ultrasonication time is not less than 10 min, and the stirring time is 3-8 h.

6. The TiMn-MOF luminescent material prepared by the method for preparing the TiMn-MOF luminescent material according to any one of claims 1 to 5.

7. The TiMn-MOF luminescent material according to claim 6, characterized in that: The TiMn-MOF luminescent material has an excitation wavelength of 350 nm and an emission wavelength of 700 nm.

Citation Information

Patent Citations

  • Fluorescent perovskite nanocrystal, and preparation method and application thereof

    CN109423278A

  • Metal organic framework Mn-MOF single-crystal material, nanosheet, preparation and application

    CN112442186A

  • Rare earth metal organic framework coated perovskite quantum dot composite luminescent material and preparation method thereof

    CN113105894A

  • Preparation method of electroluminescent sensor for detecting microcystin LR

    CN115096962A

  • Titanium heterometallic metal-organic solids, method for obtaining them and their uses

    US20210261577A1