Thermochromic composite film and preparation method thereof

By combining cellulose nanocrystals with VO2@SiO2, the weather resistance and stability of thermochromic composite films were improved, solving the problems of existing VO2 materials in smart window applications and achieving higher mechanical strength and stability.

CN118955974AActive Publication Date: 2024-11-15SICHUAN KAIGAN CARBON NANOTECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411228025.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

Existing temperature-sensitive color films made from VO2 materials cannot simultaneously achieve both weather resistance and stability when applied to smart windows.

Method used

A thermochromic composite film was prepared by combining cellulose nanocrystals with VO2@SiO2, and by modifying the cellulose nanocrystals and coating them with SiO2. This enhanced the mechanical strength and stability of the film and improved the interfacial interaction.

Benefits of technology

It improves the mechanical strength and stability of thermochromic composite membranes, enhances their adhesion to the film-forming matrix, isolates harmful external substances, and improves the stability of VO2.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of phase change materials, in particular to a thermochromic composite film and a preparation method thereof.The thermochromic composite film is formed through film liquid curtain coating, and the preparation method of the film liquid comprises the step that cellulose nanocrystals and VO2-coated SiO2 are dispersed in a film forming substrate to obtain the film liquid. The inherent rigidity, the space supporting property, the biocompatibility and the optical property of the cellulose nanocrystal are utilized, the cellulose nanocrystal is applied to the composite film, and the mechanical strength, the thermochromic property and the stability of the composite film can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phase change materials, in particular to a thermochromic composite film and a preparation method thereof. Background Art

[0002] Thermochromic materials refer to specific substances that change their color when sensing changes in the external environment temperature. That is, when the temperature is higher or lower than a certain temperature range, the color can change reversibly with the rise and fall of temperature. The temperature when the color changes is called the color change temperature. Using this characteristic of thermochromic materials, it is applied to smart windows, sensors, solar collectors, medical and other fields.

[0003] VO2 is a typical thermochromic material. Its reversible metal-semiconductor phase transition is used to change its transmittance from high transmittance at low temperature to high reflectivity at high temperature. This thermochromic (thermochromic) property makes it widely used in smart windows. One of the main preparation methods of VO2 smart windows is to compound VO2 nanopowder with polymer materials to form a film or coating. When VO2 is used in smart windows, higher requirements are placed on the weather resistance and stability of the smart windows. Summary of the invention

[0004] Technical problems solved by the present invention:

[0005] It is used to solve the problem that the existing temperature-sensitive and temperature-color films made of VO2 materials cannot take into account both weather resistance and stability when applied to smart windows.

[0006] The technical solution adopted by the present invention is:

[0007] In view of the above technical problems, the purpose of the present invention is to provide a thermochromic composite film and a preparation method thereof. The specific contents are as follows:

[0008] First, the present invention provides a thermochromic composite film, including a film layer and a thermochromic coating coated on the surface of the film layer; the preparation method of the thermochromic coating film liquid is that cellulose nanocrystals and VO2@SiO2 are dispersed in a film-forming matrix to obtain a film liquid.

[0009] In the above, the preparation method of the liquid coated with the thermochromic coating is:

[0010] (1) Preparation of VO2@SiO2: After VO2 is dispersed in ethanol, 30% NH3·H2O is added to form a first dispersion; the ratio of VO2: ethanol: NH3·H2O in the first dispersion is 1g: 150-200ml: 6-10ml; tetraethyl orthosilicate is dispersed in ethanol to form a second dispersion; the ratio of tetraethyl orthosilicate: ethanol in the second dispersion is 1g: 10ml; the second dispersion is added dropwise to the first dispersion, V (first dispersion): V (second dispersion) = 10: 1, and the addition is done slowly, and the mixture is reacted at room temperature for 10-15h. After the reaction is completed, the mixture is centrifuged, washed with deionized water, washed with anhydrous ethanol, and then dried to obtain VO2@SiO2.

[0011] (2) Cellulose nanocrystal modification:

[0012] The cellulose nanocrystals are dispersed in a solvent (the solvent is pyridine) by ultrasonic dispersion to obtain a treatment liquid. An anhydride solution (the anhydride is dodecenyl succinic anhydride and the solvent is pyridine) is added dropwise to the treatment liquid under a nitrogen atmosphere. The anhydride accounts for 2-10 wt % of the cellulose nanocrystals. After treatment at 75-95° C. for 3-7 h, the product is precipitated with distilled water and then treated with distilled water and acetone aqueous solution (V 丙酮 :V 水 =1:1) and after washing, modified cellulose nanocrystals were obtained.

[0013] (3) Preparation of membrane solution:

[0014] The film-forming matrix is ​​obtained by mixing polyvinyl alcohol and polyurethane, and modified cellulose nanocrystals and VO2@SiO2 are added to the film-forming matrix and dispersed by ultrasonic. The mass ratio of polyvinyl alcohol, polyurethane, modified cellulose nanocrystals and VO2@SiO2 is 3-7:3-7:1-3:3-10.

[0015] The technical mechanism adopted by the present invention and the beneficial effects achieved are:

[0016] (1) The thermochromic composite film provided by the present invention utilizes the intrinsic rigidity, spatial support, biocompatibility and optical properties of cellulose nanocrystals and applies them to the composite film, thereby improving the mechanical strength, thermochromic performance and stability of the composite film.

[0017] (2) The thermochromic composite film provided by the present invention is modified by treating cellulose nanocrystals, that is, grafting long carbon chains, which can increase the hydrophobicity while enhancing the binding force between the modified carboxyl groups and the nanoparticles. The improvement of hydrophobicity can enhance the interfacial interaction between the cellulose nanocrystals and the film-forming matrix.

[0018] (3) The thermochromic material provided by the present invention coats VO2 with SiO2 to isolate VO2 from adverse substances (such as oxygen, water vapor, etc.) in the outside world, thereby improving the stability of VO2. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0020] <Example>

[0021] Example 1

[0022] This embodiment provides a method for preparing a thermochromic composite film, comprising the following steps:

[0023] (1) Preparation of VO2@SiO2: 1g VO2 was dispersed in 150ml ethanol, and then ultrasonically dispersed for 15min. Then, 6ml of 30% NH3·H2O was added to form a first dispersion. 1g tetraethyl orthosilicate was dispersed in 10ml ethanol and ultrasonically dispersed to form a second dispersion. The second dispersion was added dropwise to the first dispersion, V(first dispersion):V(second dispersion)=10:1, and the mixture was slowly added dropwise. After the addition was completed, the mixture was reacted at room temperature for 15h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, washed with anhydrous ethanol, and then dried to obtain VO2@SiO2.

[0024] (2) Cellulose nanocrystal modification:

[0025] Cellulose nanocrystals are dispersed in pyridine by ultrasonic dispersion to obtain a treatment solution; then, an acid anhydride solution (the acid anhydride is dodecenylsuccinic anhydride and the solvent is pyridine) is added dropwise to the treatment solution under a N2 atmosphere, the acid anhydride accounting for 5wt% of the cellulose nanocrystals, and the product is precipitated with distilled water and then treated with distilled water and acetone aqueous solution (V 丙酮 :V 水 =1:1) and after washing, modified cellulose nanocrystals were obtained.

[0026] (3) Preparation of membrane solution:

[0027] Polyvinyl alcohol was dissolved in deionized water and heat-treated at 80°C to form a polyvinyl alcohol solution with a mass concentration of 20%. Then, the polyvinyl alcohol solution was mixed with polyurethane with a solid content of 30wt% to obtain a film-forming matrix; the VO2@SiO2 prepared by (1) and the modified cellulose nanocrystals prepared by (2) were added to the film-forming matrix, and then ultrasonically dispersed to obtain a film liquid. The mass ratio of polyvinyl alcohol, polyurethane, modified cellulose nanocrystals and VO2@SiO2 was 5:5:3:7. After vacuum degassing, the film liquid was cast and the film thickness was controlled at 150μm. Its visible light transmittance was 69.4%, the phase transition temperature was 48°C, and the thermal insulation performance was △=6°C. After an aging test at 60°C and 90%, the enthalpy value of 72h was measured to be 12.7J / g.

[0028] Example 2

[0029] The difference between this embodiment and embodiment 1 is that the mass ratio of polyvinyl alcohol, polyurethane, modified cellulose nanocrystals, and VO2@SiO2 is 5:5:1:9. The film thickness is controlled at 150 μm, its visible light transmittance is 68.7%, the phase transition temperature is 48°C, and the thermal insulation performance is △=6°C. After an aging test at 60°C and 90%, the enthalpy value of 72h was measured to be 12.4 J / g.

[0030] <Comparative Example>

[0031] Comparative Example 1

[0032] The difference between this comparative example and Example 1 is that cellulose nanocrystals are not added. The film thickness is controlled at 150 μm, its visible light transmittance is 62.1%, the phase transition temperature is 54°C, and the thermal insulation performance is △=3°C. After an aging test at 60°C and 90%, the enthalpy value at 72h is measured to be 9.6 J / g.

[0033] Comparative Example 2

[0034] The difference between this comparative example and Example 1 is that the modified cellulose nanocrystals are replaced by cellulose nanocrystals. The film thickness is controlled at 150 μm, its visible light transmittance is 66.7%, the phase transition temperature is 50°C, and the thermal insulation performance is △=5°C. After an aging test at 60°C and 90%, the enthalpy value at 72h is measured to be 11.4 J / g.

[0035] Comparative Example 3

[0036] The difference between this comparative example and Example 1 is that VO2@SiO2 is replaced by VO2. The film thickness is controlled at 150μm, its visible light transmittance is 59.4%, the phase transition temperature is 55℃, and the thermal insulation performance is △=4℃. After an aging test at 60℃ and 90%, the enthalpy value of 72h is measured to be 11.1J / g.

[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thermochromic composite film, characterized in that: The membrane is formed by casting a membrane liquid, and the preparation method of the membrane liquid is that cellulose nanocrystals and VO2@SiO2 are dispersed in a membrane-forming matrix to obtain the membrane liquid.

2. The thermochromic composite film according to claim 1, characterized in that: The preparation method of the membrane solution comprises the following steps: (1) Preparation of VO2@SiO2; (2) Modification of cellulose nanocrystals; (3) Add modified cellulose nanocrystals and VO2@SiO2 into the film-forming matrix and disperse them to obtain a membrane liquid.

3. The thermochromic composite film according to claim 2, characterized in that: (1), VO2 is dispersed in ethanol, and then NH3·H2O is added to form a first dispersion; tetraethyl orthosilicate is dispersed in ethanol to form a second dispersion; the second dispersion is added dropwise to the first dispersion, and after the addition, the dispersion is reacted at room temperature. After the reaction is completed, the dispersion is centrifuged, washed, and then dried to obtain VO2@SiO2.

4. The thermochromic composite film according to claim 3, characterized in that: (1) includes at least one of features (1-1) to (1-4): (1-1) In the first dispersion, the ratio of VO2: ethanol: NH3·H2O is 1 g: 150-200 ml: 6-10 ml; (1-2) The ratio of tetraethyl orthosilicate to ethanol in the second dispersion is 1 g:10 ml; (1-3) V(first dispersion):V(second dispersion)=10:1; (1-4) The reaction time is 10 to 15 hours.

5. The thermochromic composite film according to claim 2, characterized in that: (3) includes at least one of features (3-1) to (3-2): (3-1) The film-forming medium includes polyvinyl alcohol and polyurethane; (3-2) The mass ratio of film-forming medium, modified cellulose nanocrystals, and VO2@SiO2 is 10:1~3:3~10.

6. The thermochromic composite film according to claim 5, characterized in that: (3) includes at least one of features (3-3) to (3-4): (3-3) Polyvinyl alcohol: a polyvinyl alcohol aqueous solution with a mass concentration of 10 to 30%; (3-4) The solid content of the polyurethane is 15 to 35%.

7. The thermochromic composite film according to any one of claims 2 to 6, characterized in that: (2), cellulose nanocrystals are dispersed in a solvent to obtain a treatment solution, an acid anhydride solution is added dropwise to the treatment solution, and the product is precipitated with distilled water after heat treatment and then washed to obtain modified cellulose nanocrystals.

8. The thermochromic composite film according to claim 7, characterized in that: (2) includes at least one of features (2-1) to (2-3): (2-1) the acid anhydride is dodecenylsuccinic anhydride; (2-2) the acid anhydride accounts for 2 to 10 wt% of the cellulose nanocrystals; (2-3) Heat treatment: 75-95°C for 3-7h.

9. The method for preparing a thermochromic composite film according to any one of claims 1 to 8, comprising the following steps: dispersing cellulose nanocrystals and VO2@SiO2 in a film-forming matrix to obtain a film liquid, vacuum degassing the film liquid, and then casting the solution into a film.

Citation Information

Patent Citations

  • Preparing method for acylated fiber nanocrystal

    CN105601754A

  • High-performance vanadium-dioxide-based thermochromism composite

    CN105694615A

  • Preparation method of self-cleaning intelligent temperature control nano-cellulose membrane, nano-cellulose membrane prepared by preparation method, and application of nano-cellulose membrane

    CN110818929A

  • Thermochromic composite material, its preparation and use

    US20220242004A1