Preparation method and application of photochromic ink

A low-cost, environmentally friendly photochromic ink was prepared by adding polyvinyl alcohol, sulfuric acid and nickel sulfate hexahydrate to sodium tungstate solution, and adding copper chloride at room temperature, which solved the existing problem. The high cost and pollution problems in the technology have achieved low-cost and environmentally friendly photochromic rendering effects, suitable for intelligent anti-counterfeiting and instantaneous display.

CN118956207AActive Publication Date: 2024-11-15WUHAN TEXTILE UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411134614.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing photochromic material preparation methods have high cost, high energy consumption, large pollution, complex operation and untimely response, and it is difficult to meet the needs of low cost, environmental protection and immediate response.

Method used

A low-cost, environmentally friendly photochromic ink is prepared by adding polyvinyl alcohol, sulfuric acid and nickel sulfate hexahydrate to sodium tungstate solution, adjusting the pH value, and adding copper chloride at room temperature. The reaction of these compounds is used to generate WO3 and other components, enhancing the absorption of ultraviolet light and the uniformity of ink.

Benefits of technology

Realizes low-cost, environmentally friendly, simple operation photochromic ink preparation, can be completed at room temperature, and color rendered and displayed repeatedly under ultraviolet lamp irradiation. It is suitable for intelligent anti-counterfeiting and instantaneous display applications without causing toxicity and harmfulness. substance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956207A_ABST
    Figure CN118956207A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of photochromic ink. The preparation method comprises the following steps: adding a small amount of polyvinyl alcohol into a sodium tungstate dihydrate solution, then adding a proper amount of sulfuric acid to adjust the pH value to 1.2-2.0 to obtain a tungstic acid solution, continuing to react and decompose to obtain WO3, and controlling the solution within the acidity range to obtain WO3 particles with smaller size. And finally, adding a small amount of cuprous chloride into the solution, stirring and reacting to obtain the photochromic ink. In the process of preparing the photochromic ink, toxic and harmful substances are not generated, and the ink is environment-friendly and pollution-free; the method can be completed in a room temperature environment, and loss of electric heating energy is not generated. The prepared photochromic ink can be used for writing and drawing on the surfaces of hydrophilic substrates such as paper and cotton cloth; after an adhesive is added into the photochromic ink, a pattern can be quickly printed by using a seal; the pattern is invisible after being dried and is displayed after being irradiated by an ultraviolet lamp. The method has great advantages in the aspects of intelligent anti-counterfeiting and instantaneous display application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photochromic ink, and in particular to a preparation method and application of photochromic ink. Background Art

[0002] In recent years, smart materials that can respond to external stimuli such as heat, light, electricity, magnetism, force, humidity and chemical input have attracted more and more attention. Among these stimuli, light, especially sunlight, has the advantages of being versatile, reproducible and available, in addition to the advantages of being easy to control parameters such as precise position, wavelength, intensity and duration of irradiation. Photochromic materials are materials that can reversibly change color under light stimulation and have been widely developed.

[0003] Generally, the excitation of photochromism requires ultraviolet radiation of a certain intensity. The ink solution prepared using photochromic materials can be completely invisible in the dried state after drawing patterns or writing, and only a very low-power ultraviolet lamp is needed to make it color. It has good applications in anti-counterfeiting and instantaneous color display. Summary of the invention

[0004] The purpose of the present invention is to provide a preparation method and application of photochromic ink with simple synthesis, low cost and instant response. The preparation method does not produce toxic and harmful substances during the preparation process, is environmentally friendly and pollution-free, and is simple to operate; it can be completed at room temperature, does not produce loss of electric heat energy, and has low cost.

[0005] To achieve the above object, the present invention provides a method for preparing a photochromic ink, comprising the following steps:

[0006] S1, preparing a sodium tungstate dihydrate solution of a predetermined concentration;

[0007] S2, adding polyvinyl alcohol to the sodium tungstate dihydrate solution, and stirring to obtain a mixed solution;

[0008] S3, adding sulfuric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.2-2.0;

[0009] S4, adding nickel sulfate hexahydrate to the solution obtained in step S3, and stirring to react;

[0010] S5, adding cuprous chloride to the solution obtained in step S4, stirring for reaction, and obtaining photochromic ink.

[0011] Furthermore, in step S5, the mass fraction of cuprous chloride is 1-4%, and the stirring reaction time is 5-10 min.

[0012] Further, in step S2, the amount of polyvinyl alcohol added is 2-10 wt%.

[0013] Furthermore, in step S1, the concentration of the sodium tungstate dihydrate solution is 0.1-0.2 mol / L, and the solvent used is ethylene glycol.

[0014] Furthermore, in step S3, the concentration of the added sulfuric acid is 2-3 mol / L.

[0015] Furthermore, in step S4, the mass fraction of the nickel sulfate hexahydrate is 10-20 wt %, and the stirring reaction time is 20-30 min.

[0016] To achieve the above-mentioned purpose, the present invention also provides an application of a photochromic ink, wherein the photochromic ink is prepared by the preparation method described in any of the technical schemes in the aforementioned technical schemes; a brush is dipped in the photochromic ink to write or draw on the surface of a hydrophilic substrate; the pattern becomes invisible after drying, and the pattern is displayed after irradiation with ultraviolet light.

[0017] Furthermore, the hydrophilic substrate is a material such as paper or cotton cloth.

[0018] To achieve the above-mentioned purpose, the present invention also provides an application of a photochromic ink, wherein the photochromic ink is prepared by the preparation method described in any of the technical schemes in the aforementioned technical schemes; after adding an adhesive to the photochromic ink, a pattern is quickly printed using a stamp; the pattern becomes invisible after drying, and the pattern is displayed after irradiation with ultraviolet light.

[0019] Furthermore, the adhesive is polyvinyl alcohol (PVA), acrylic resin, epoxy resin, etc.

[0020] The beneficial effects of the present invention are:

[0021] 1. The preparation method of the photochromic ink provided by the present invention is to add a small amount of polyvinyl alcohol (PVA) to a sodium tungstate dihydrate solution, and then add an appropriate amount of sulfuric acid to adjust the pH to 1.2-2.0. Sodium tungstate (Na2WO4) reacts with sulfuric acid (H2SO4) to generate tungstic acid (H2WO4) and sodium sulfate (Na2SO4). In this process, sulfuric acid provides an acidic environment, so that the tungstate ions in the sodium tungstate combine with hydrogen ions to generate tungstic acid precipitation. Continue to react and decompose to obtain WO3, and the WO3 particles obtained by controlling the solution within the acidic range are smaller in size, so that its absorption of ultraviolet light energy is enhanced, and the obtained ink has better uniformity. Then nickel sulfate hexahydrate is added for reaction, and finally a small amount of cuprous chloride is added to the solution for stirring and reaction, so as to obtain photochromic ink. In the process of preparing the photochromic ink of the present invention, no toxic and harmful substances are generated, it is environmentally friendly and pollution-free, and the operation is simple; and it can be completed at room temperature, without generating loss of electric heating energy, and the cost is low.

[0022] 2. The photochromic ink prepared by the present invention can be used to draw any pattern on erasable substrates such as ordinary paper and cotton fabrics, and the pattern drawn becomes invisible after the ink is air-dried. When irradiated with ultraviolet light, the pattern can be displayed instantly, and it can remain invisible after being switched on and off many times. Experiments show that the display behavior can be repeated more than a thousand times. It has great advantages in intelligent anti-counterfeiting and instantaneous display applications.

[0023] 3. The photochromic ink prepared by the present invention can not only display color and fade instantly, but also can display the pattern and retain it for a certain period of time under long-term ultraviolet light irradiation, and the time is related to the length of ultraviolet light irradiation. It can also fade and become invisible under dark / indoor natural conditions, and has good repeated display performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a photograph of English letters written on paper using the photochromic ink prepared in Example 1, displayed under ultraviolet light.

[0025] Figure 2 This is a photograph of the photochromic ink prepared in Example 1 drawn on paper, showing a real object under ultraviolet light.

[0026] Figure 3 This is a real-life diagram of the instantaneous display cycle of the ink in Example 1.

[0027] Figure 4 This is a physical image of the pattern drawn by the ink in Example 1 under strong ultraviolet irradiation.

[0028] Figure 5 This is a real picture of the effect of printing a pattern on paper using ink without adding PVA in comparative example 1.

[0029] Figure 6 This is a real picture of the ink stability test of comparative example 2 without adding NiSO4·6H2O.

[0030] Figure 7 This is the display diagram of the ink of comparative example 3 without adding CuCl after ultraviolet irradiation.

[0031] Figure 8 The following are photos of the inks prepared in Example 1 (left) and Comparative Example 3 (right). DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0034] The present invention provides a method for preparing a photochromic ink, comprising the following steps:

[0035] S1, preparing a sodium tungstate dihydrate solution of a predetermined concentration;

[0036] The concentration of sodium tungstate dihydrate solution is 0.1-0.2 mol / L, the solvent used is ethylene glycol, and stirring is performed for 5-10 minutes.

[0037] S2, adding a small amount of polyvinyl alcohol to the sodium tungstate dihydrate solution, stirring evenly to obtain a mixed solution;

[0038] The amount of polyvinyl alcohol added is 2-10 wt%, and stirring is performed for 10-15 minutes.

[0039] S3, adding sulfuric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.2-2.0;

[0040] The concentration of the added sulfuric acid is 2-3 mol / L, and stirring is continued for 10-15 minutes.

[0041] S4, adding nickel sulfate hexahydrate to the solution obtained in step S3, and stirring the solution for reaction; the mass fraction of nickel sulfate hexahydrate is 10-20wt%, and the stirring reaction time is 20-30min.

[0042] S5, adding cuprous chloride to the solution obtained in step S4, stirring for reaction, and obtaining photochromic ink.

[0043] The mass fraction of cuprous chloride is 1-4%, and the stirring reaction time is 5-10 minutes.

[0044] The present invention also provides the application of the photochromic ink prepared according to the above-mentioned preparation method; after dipping the photochromic ink with a brush, writing or drawing is performed on the surface of a hydrophilic substrate; after drying, the pattern is invisible, and after irradiation with ultraviolet light, the pattern is displayed, responds promptly and can be displayed repeatedly.

[0045] Among them, the hydrophilic substrate is a material such as paper or cotton cloth.

[0046] It is also possible to add an adhesive to the photochromic ink and then quickly print a pattern using a stamp; the pattern becomes invisible after drying and is displayed after being irradiated with an ultraviolet light, responding promptly and being able to be displayed repeatedly.

[0047] Among them, the adhesive is polyvinyl alcohol (PVA), acrylic resin, epoxy resin, etc.

[0048] The preparation method of the photochromic ink provided by the present invention is described below with reference to specific embodiments.

[0049] Example 1

[0050] This embodiment provides a method for preparing a photochromic ink, comprising the following steps:

[0051] S1, prepare a 0.1 mol / L sodium tungstate dihydrate solution with ethylene glycol and stir for 5 min;

[0052] S2, adding 2 wt % polyvinyl alcohol (PVA) to the sodium tungstate dihydrate solution prepared in step S1 and stirring for 15 min to obtain a mixed solution;

[0053] S3, adding 2 mol / L sulfuric acid to the mixed solution obtained in step S2 to adjust the pH to 1.2;

[0054] S4, adding 20 wt% nickel sulfate hexahydrate (NiSO4·6H2O) to the solution obtained in step S3, and stirring the mixture for 20 min;

[0055] S5, adding 2 wt % cuprous chloride to the solution obtained in step S4 and stirring the mixture for 5 minutes to obtain a photochromic ink.

[0056] A small amount of polyvinyl alcohol (PVA) is added to the sodium tungstate dihydrate solution, and then an appropriate amount of sulfuric acid is added to adjust the pH to 1.2-2.0. Sodium tungstate (Na2WO4) reacts with sulfuric acid (H2SO4) to generate tungstic acid (H2WO4) and sodium sulfate (Na2SO4). In this process, sulfuric acid provides an acidic environment, so that the tungstate ions in the sodium tungstate combine with hydrogen ions to generate tungstic acid precipitation. Continue to react and decompose to obtain WO3. The WO3 particles obtained by controlling the solution within this acidic range are smaller in size, so that its absorption of ultraviolet light energy is enhanced, and the obtained ink has better uniformity. Then nickel sulfate hexahydrate is added to react, and finally a small amount of cuprous chloride is added to the solution and stirred to react, and a photochromic ink is obtained.

[0057] The prepared photochromic ink can be used for writing and drawing on the surface of hydrophilic substrates such as paper and cotton cloth; the pattern is invisible after drying and is visible after irradiation with ultraviolet light.

[0058] It is also possible to add an adhesive to the photochromic ink and use a stamp to quickly print a pattern; the pattern becomes invisible after drying and is revealed after exposure to ultraviolet light.

[0059] See also Figure 1 , Figure 2The photo is a photo of English letters / patterns written on paper by the photochromic ink prepared in Example 1, and displayed under ultraviolet light. As can be seen from the figure, the letters / patterns are invisible after being written and air-dried on the paper, and only become visible when irradiated with ultraviolet light.

[0060] See also Figure 3 , Figure 4 As shown, it is a physical picture of the pattern cycle display / color retention drawn by the ink in Example 1, by Figure 3 It can be seen that the pattern drawn by the color-changing ink can remain invisible after being irradiated by ultraviolet light for many times, and the color display can be repeated more than a thousand times. The photochromic ink has great advantages in intelligent anti-counterfeiting and instantaneous display applications.

[0061] Figure 4 It can be seen that after the pattern drawn with the ink is exposed to strong UV light, the pattern display can be retained for more than 72 hours, and the color will fade after 4-5 days, but the pattern can still be displayed after being exposed again.

[0062] Comparative Example 1

[0063] Comparative Example 1 provides a method for preparing a photochromic ink. Compared with Example 1, the difference is that in step S2, PVA is not added. The rest is substantially the same as Example 1 and will not be described again.

[0064] Experiments show that not adding PVA has little effect on the stability of the solution. However, due to the strong fluidity of the solution, it is easy to smudge when writing or drawing on the surface of fabric / paper. Figure 5 shown.

[0065] Comparative Example 2

[0066] Comparative Example 2 provides a method for preparing a photochromic ink. Compared with Example 1, the difference is that in step S4, NiSO4·6H2O is not added. The rest is substantially the same as Example 1 and will not be described again.

[0067] Experiments show that compared with the photochromic ink prepared in Example 1, the stability of the solution system is reduced, and particles are easily deposited after being placed for 12 hours, such as Figure 6 shown.

[0068] Comparative Example 3

[0069] Comparative Example 3 provides a method for preparing a photochromic ink. Compared with Example 1, the difference is that in step S5, CuCl is not added. The rest is substantially the same as Example 1 and will not be described again.

[0070] Experiments show that the solution has good stability, but if the ultraviolet power is strong, the color will be retained directly and the recovery will be slow, such as Figure 7shown.

[0071] See also Figure 8 The following are photos of the inks prepared in Example 1 (left) and Comparative Example 3 (right). It can be seen from the figure that the color of the solution with CuCl added is blue-black, while the color of the solution without CuCl added is cyan. This is because the added Cu + After WO3 is reduced, the blue state of WO3 is displayed.

[0072] Comparative Example 4

[0073] Comparative Example 4 provides a method for preparing a photochromic ink. Compared with Example 1, the difference is that in step d, NiSO4·6H2O is not added; in step e, CuCl is not added. The rest is substantially the same as Example 1 and will not be described again.

[0074] Without adding any dopants, the stability of pure tungstic acid solution is poor. After being left for 2 to 3 hours, the solution is easy to settle. It can be used as ink for writing and can be air-dried to become invisible. However, it will leave traces after being exposed to ultraviolet light and it will take a long time to recover.

[0075] Examples 2-6 and Comparative Examples 5-7

[0076] The preparation methods of the photochromic inks provided in Examples 2-6 and Comparative Examples 5-7 are different from those in Example 1 in that the mass fraction of PVA in step S2, the value of adjusting the pH in step S3, the mass fraction of NiSO4·6H2O in step S4, and the mass fraction of cuprous chloride in step S5 are changed, as shown in the following table; the rest are roughly the same as in Example 1 and will not be repeated here.

[0077]

[0078] Comparison of Examples 1-3 shows that as the mass fraction of the added PVA increases, the stability of the ink increases. Compared with high-concentration PVA, low-content PVA is more beneficial in improving the writing and printability of the ink. However, when the mass fraction is greater than 10wt% (Comparative Example 5), the viscosity of the ink is too high to be conducive to printing patterns, and the drying of the pattern after writing is prone to leave traces.

[0079] Comparison of Examples 1 and 6 with Comparative Examples 6-7 shows that CuCl has good reducing properties and plays an important role in improving the color reduction of solution particles. However, when the CuCl content is too low, the improvement of its fading ability is not obvious, and when the CuCl content is too high, the fading ability of the solution particles is not obvious. + The W ions of WO3 in the system are reduced and directly displayed as blue-black ink. After a period of time, a large amount of Cu 2+ The presence of ions has an adverse effect on the stability of the solution.

[0080] In summary, the preparation method of the photochromic ink provided by the present invention is to add a small amount of polyvinyl alcohol (PVA) to a sodium tungstate dihydrate solution, and then add an appropriate amount of sulfuric acid to adjust the pH to 1.2-2.0 to obtain tungstic acid, which is easily decomposed to form WO3, and the WO3 particles obtained in the solution within the acidic range are smaller in size, so that its absorption of ultraviolet light energy is enhanced, and the obtained ink has better uniformity. Then nickel sulfate hexahydrate is added for reaction, and finally a small amount of cuprous chloride is added to the solution for stirring and reaction, so as to obtain a photochromic ink. In the process of preparing the photochromic ink of the present invention, no toxic and harmful substances are produced, the invention is environmentally friendly and pollution-free, and the operation is simple; and it can be completed at room temperature, without generating loss of electric heating energy, and the cost is low. It has great advantages in intelligent anti-counterfeiting and instantaneous display applications.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a photochromic ink, characterized in that: The following steps are involved: S1, preparing a sodium tungstate dihydrate solution of a predetermined concentration; S2, adding polyvinyl alcohol to the sodium tungstate dihydrate solution, and stirring to obtain a mixed solution; S3, adding sulfuric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.2-2.0; S4, adding nickel sulfate hexahydrate to the solution obtained in step S3, and stirring to react; S5, adding cuprous chloride to the solution obtained in step S4, stirring for reaction, and obtaining photochromic ink.

2. The method for preparing the photochromic ink according to claim 1, characterized in that: In step S5, the mass fraction of cuprous chloride is 1-4%, and the stirring reaction time is 5-10 minutes.

3. The method for preparing the photochromic ink according to claim 1, characterized in that: In step S2, the amount of polyvinyl alcohol added is 2-10 wt%.

4. The method for preparing the photochromic ink according to claim 1, characterized in that: In step S1, the concentration of the sodium tungstate dihydrate solution is 0.1-0.2 mol / L, and the solvent used is ethylene glycol.

5. The method for preparing the photochromic ink according to claim 1, characterized in that: In step S3, the concentration of the added sulfuric acid is 2-3 mol / L.

6. The method for preparing the photochromic ink according to claim 1, characterized in that: In step S4, the mass fraction of nickel sulfate hexahydrate is 10-20 wt %, and the stirring reaction time is 20-30 min.

7. An application of a photochromic ink, characterized in that: The photochromic ink is prepared according to the preparation method according to any one of claims 1 to 6; a brush is dipped in the photochromic ink to write or draw on the surface of a hydrophilic substrate; the pattern becomes invisible after drying, and becomes visible after irradiation with ultraviolet light.

8. The use of the photochromic ink according to claim 7, characterized in that: The hydrophilic substrate is paper or cotton cloth.

9. An application of a photochromic ink, characterized in that: The photochromic ink is prepared according to the preparation method according to any one of claims 1 to 6; after adding an adhesive to the photochromic ink, a pattern is quickly printed using a stamp; the pattern is invisible after drying, and is displayed after irradiation with ultraviolet light.

10. The use of the photochromic ink according to claim 9, characterized in that: The adhesive is polyvinyl alcohol, acrylic resin or epoxy resin.

Citation Information

Patent Citations

  • Polytungstate-hydrotalcite composite photochromic ultrathin film and preparation method thereof

    CN102876316A

  • Preparation method of composite WO3 sol and composite WO3 sol prepared by preparation method

    CN108083340A

  • Preparation method of WO3 with microsphere-shaped and flower-shaped composite morphology

    CN110627124A

  • Ultra-small inorganic nano heterojunction photochromic material, erasable rewritable medium prepared from material, and preparation method of erasable rewritable medium

    CN111944512A

  • Photochromic complex

    JP2019137796A