Method for improving loess by using biomass ash content
The biomass ash treated with calcination and grinding is mixed with other substances to improve the loess, which solves the problems of insufficient compressive strength and poor durability of the loess, significantly improves its compressive strength and durability, and enhances the stability of the soil structure.
Patent Information
- Application Number
- CN202411013909.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
Loess is prone to compression deformation and damage when subjected to external forces, resulting in insufficient compressive strength and poor durability, which affects the bearing capacity and engineering safety of roads and foundations.
By calcining biomass ash (such as rice husk ash) at high temperature and mixing it with vermiculite, methyl laurate, liquid paraffin and other substances, it forms improved loess, enhances the particle binding force and structural density of loess, and improves compressive strength and Durability.
It significantly improves the compressive strength and durability of loess, can better resist the influence of traffic loads and natural environmental factors, and enhances the stability and physical properties of soil structure.
Smart Images

Figure BDA0004965155120000081 
Figure BDA0004965155120000082 
Figure BDA0004965155120000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of soil improvement, and more specifically, to a method for improving loess by utilizing biomass ash. Background Art
[0002] As a widely distributed geological material, loess has important application value in the field of civil engineering, especially in road construction and foundation treatment. However, in practical applications, due to the weak bonding force between loess particles and the developed pore structure, it is easy to be compressed and deformed and damaged when subjected to external forces, resulting in a decrease in the bearing capacity of the roadbed and foundation, affecting the safety and durability of the project. Especially under the combined effects of traffic loads and natural environmental factors (such as rainwater erosion, freeze-thaw cycles, etc.), the compressive strength problem of loess is more prominent, becoming one of the key factors restricting the application of loess engineering.
[0003] Therefore, it is particularly urgent to find an effective improvement method to address the problems of insufficient compressive strength and poor durability of loess. Summary of the invention
[0004] In order to improve the compressive strength and durability of improved loess, the present application provides a method for improving loess using biomass ash.
[0005] In the first aspect, the present application provides a method for improving loess using biomass ash, which adopts the following technical solution: A method for improving loess using biomass ash comprises the following steps: (1) calcining the biomass ash at 500-600° C. for 60-90 min, taking it out, and grinding it at 200-250 r / min for 30-40 min to obtain pretreated biomass ash; (2) taking the pretreated biomass ash and mixing it with vermiculite, methyl laurate, liquid paraffin and loess, sprinkling water while stirring, and after mixing evenly, sealing and placing for 18-24 hours to obtain improved loess; the biomass ash is rice husk ash.
[0006] By adopting the above technical solution, the minerals such as silicon dioxide and aluminum oxide rich in rice husk ash have a more stable structure through high-temperature calcination, and the calcination and grinding treatment further refines the particles, which can form a denser microstructure after mixing with loess, thereby improving the compressive strength of loess. At the same time, calcination and grinding increase the surface area and reaction activity of rice husk ash, so that it can better react chemically with substances in loess to form aluminosilicates, etc., enhance the bonding force between loess particles, reduce weathering caused by water erosion, and thus improve the durability of loess.
[0007] Pretreated rice husk ash, vermiculite, methyl laurate, liquid paraffin and loess are mixed in a certain proportion, and water is sprinkled and stirred to ensure that the components are evenly distributed; sealing and placement further promotes the interaction and fusion of these components, significantly enhancing the improvement effect of loess and improving soil structure.
[0008] Optionally, in the improved loess raw material, the added amount of each raw material is as follows: 80-100 parts of loess, 8-10 parts of rice husk ash, 8-10 parts of liquid paraffin, 0.5-0.8 parts of methyl laurate, 1-2 parts of vermiculite and 20-25 parts of water.
[0009] By adopting the above technical solution, rice husk ash, as a natural siliceous material, is rich in silicon dioxide, and its fine particles effectively fill the gaps between loess particles to form a tighter structural foundation. At the same time, the alkaline components in rice husk ash can also react with certain components in loess to promote soil hardening and significantly improve the strength of loess. Liquid paraffin can penetrate between loess particles, not only playing a lubricating role, wrapping the loess so that the surface of the loess gradually changes from rough to smooth, but also by reducing the porosity, it enhances the close arrangement of loess particles. More importantly, it replaces the role of water in the pores, ensures the compaction of loess, and forms a protective film on the surface of loess with its own waterproof properties, effectively resisting water erosion and further strengthening the loess structure.
[0010] Methyl laurate, as an organic ester compound, has good waterproof properties. Its trace addition can effectively prevent water penetration and reduce loess cracking caused by dry-wet and freeze-thaw cycles, thereby enhancing the stability of loess. Vermiculite has good water absorption and water retention properties and a stable structure. And because of its characteristic of swelling when exposed to water, it can regulate the humidity changes of loess to a certain extent, reduce the volume changes caused by water fluctuations, and further enhance the stability of loess.
[0011] These raw materials work together to build a multi-dimensionally enhanced loess structural system. The hardening of rice husk ash, the waterproofing and lubricating properties of liquid paraffin, the waterproofing and cracking resistance of methyl laurate, and the regulating function of vermiculite complement each other, jointly solving the problems of insufficient strength and poor durability of loess, and significantly improving the comprehensive performance of loess, enabling it to better resist the long-term influence of external environmental factors and maintain the stability of physical properties.
[0012] Optionally, the loess is dried at 100-110° C. to constant weight, crushed and passed through a 2-5 mm sieve.
[0013] By adopting the above technical solution, the loess particles are further refined by crushing to make their particle size distribution more uniform. At the same time, the composition of the loess is homogenized and impurities therein are removed. The refined loess particles increase the specific surface area, which is conducive to more sufficient contact and reaction with the modified components.
[0014] Optionally, the rice husk ash is further subjected to a modification operation after the pretreatment operation, and the modification steps are as follows: S1. Dissolve the calcined rice husk ash in anhydrous ethanol, add amino silicone oil while stirring, react in a constant temperature water bath at 60-90° C. for 8-9 hours, wash, filter, and dry to obtain preliminarily modified rice husk ash for later use; S2, take polyphenylene sulfide and p-chlorobenzoic acid, sodium hydroxide, 1-methyl-pyrrolidone, pass nitrogen protection, stir evenly, heat to 220-250°C at a rate of 1-3°C / min, keep warm for 3-4h, then cool to 200-220°C at the same rate, keep warm for 20-30min, and finally cool to 120-140°C at the same rate, filter, wash and dry to obtain modified polyphenylene sulfide; S3. Disperse the modified polyphenylene sulfide in anhydrous toluene, add the rice husk ash preliminarily modified in S1, and then add acetic acid, react at 90-110°C for 10-12h, filter, wash, and extract with ethanol solution for 24h, and vacuum dry to constant weight to obtain modified rice husk ash.
[0015] By adopting the above technical scheme, the amino silicone oil is hydrolyzed, and the silicon-oxygen bonds therein react with the hydroxyl groups on the surface of the rice husk ash to form covalent bonds. Small molecule organic matter with amino groups is grafted onto the surface of the rice husk ash and reacts with the carboxyl-modified polyphenylene sulfide. The polyphenylene sulfide has high rigidity and high bending modulus, and good creep resistance under load. A stable composite material structure is formed on the surface of the rice husk ash particles through the modification reaction, which enhances the bonding force between the rice husk ash and the loess particles, so that the improved loess can better resist deformation and damage when subjected to external forces, thereby further improving the compressive strength of the improved loess.
[0016] Optionally, the weight ratio of rice husk ash to amino silicone oil in S1 is 1:2.8-4.2.
[0017] By adopting the above technical scheme, it can be ensured that the hydroxyl groups on the surface of rice husk ash are fully in contact with and react with the silicon-oxygen bonds or amino functional groups in the amino silicone oil, thereby achieving the preliminary modification of the rice husk ash particles.
[0018] Optionally, the weight ratio of the modified polyphenylene sulfide and the preliminarily modified rice husk ash added in S3 is 0.8-1.2:1.
[0019] Optionally, the raw materials also include 1-3 parts of calcium sulphoaluminate.
[0020] By adopting the above technical solution, the calcium sulphoaluminate hydrate crystals will gradually fill the pores and cracks between loess particles during the formation process. This filling effect significantly reduces the porosity of the soil and improves the density and compressive strength of the soil. In addition, the interweaving and overlapping between these crystals build a more solid network structure, further enhancing the overall structural strength of the soil, making it show more excellent performance in engineering applications.
[0021] In a second aspect, the present application provides an application of improved loess prepared by the present method in engineering fillers.
[0022] In summary, this application has the following beneficial effects: 1. Due to the synergistic effect of the raw materials in this application, a multi-dimensional enhanced loess structure system is constructed through the hardening of rice husk ash, the waterproof and lubricating function of liquid paraffin, the waterproof and anti-cracking function of methyl laurate, and the regulating function of vermiculite, thereby improving the compressive strength and durability of loess.
[0023] 2. The present application obtains highly active rice husk ash by reasonably controlling the calcination temperature and calcination time through the calcination treatment of rice husk ash, thereby preventing the precipitation of impurities and metals inside the rice husk ash from adversely affecting the improved loess. Further, the highly active rice husk ash can better play an improvement effect, improve the internal structure of loess, and help improve the compressive strength and durability of the improved loess.
[0024] 3. In this application, carboxyl-modified polyphenylene sulfide is added to modify the rice husk ash. As a polymer material, modified polyphenylene sulfide has high rigidity and creep resistance, and can provide additional strength and stability for the rice husk ash. The modified rice husk ash is added to the loess to better optimize the structure, provide good support, and improve the compressive strength of the improved loess.
[0025] 4. The method of the present application utilizes agricultural waste rice husks and converts them into high-value modified rice husk ash through modification, thereby achieving effective utilization of resources and reduction, harmlessness and resource utilization of waste, and has significant environmental significance. DETAILED DESCRIPTION
[0026] The present application is further described in detail below with reference to the embodiments.
[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0028] Rice husk ash is used as biomass ash in this application, wherein the contents of the components are as follows: SiO2 87.20%, Al2O3 0.15%, Fe2O3 0.16%, CaO 0.55%, MgO 0.35%, SO3 0.24%, Na2O 1.12%, K2O3.68% and unburned carbon; The main chemical components of loess are SiO2 62.11%, Al2O3 12.35%, CaO 3.36%, Fe2O35.62%, MgO2.65%, K2O 2.41%, Na2O 2.04%, SO3 0.12%, and loss on ignition 9.34%; Paraffin oil was purchased from Shandong Yousuo Chemical Technology Co., Ltd., item number 4100511, No. 5 white oil, a mixture of C16-C31 normal isomers; polyphenylene sulfide powder was purchased from Dongguan Xinrui New Materials Co., Ltd., 800 mesh. Example
[0029] Example 1 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 500° C. for 75 min, and then ground at 225 r / min for 30 min to obtain pretreated rice husk ash; (2) 10 kg of pretreated rice husk ash, 1 kg of vermiculite, 0.8 kg of methyl laurate, 9 kg of liquid paraffin and 90 kg of loess were mixed, and 22 kg of water was sprinkled into the mixture while stirring. After stirring and mixing evenly, the mixture was sealed and placed for 24 hours to obtain the improved loess.
[0030] An application of improved loess comprises the following steps: (1) The prepared improved loess is transported to the site and filled in layers. After each layer of engineering soil filling is completed, a heavy-duty earth compactor is used for static compaction; (2) After the engineering soil filling is completed in layers, it is mechanically vibrated and compacted, and then filled and leveled to form an improved loess foundation.
[0031] Example 2 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 550° C. for 60 min, and then ground at 250 r / min for 35 min to obtain pretreated rice husk ash; (2) 8 kg of pretreated rice husk ash, 1.5 kg of vermiculite, 0.5 kg of methyl laurate, 10 kg of liquid paraffin and 100 kg of loess were mixed, and 20 kg of water was sprinkled into the mixture while stirring. After stirring and mixing evenly, the mixture was sealed and placed for 20 hours to obtain the improved loess; the biomass ash was rice husk ash.
[0032] An application of improved loess, same as Example 1.
[0033] Example 3 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 600° C. for 90 min, and then ground at 200 r / min for 40 min to obtain pretreated rice husk ash; (2) 8 kg of pretreated rice husk ash, 1.5 kg of vermiculite, 0.5 kg of methyl laurate, 10 kg of liquid paraffin and 100 kg of loess were mixed, and 20 kg of water was sprinkled into the mixture while stirring. After stirring and mixing evenly, the mixture was sealed and placed for 18 hours to obtain the improved loess; the biomass ash was rice husk ash.
[0034] An application of improved loess, same as Example 1.
[0035] Example 4 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 500° C. for 75 min, and then ground at 225 r / min for 30 min to obtain pretreated rice husk ash; (2) Modified rice husk ash: S1, take 10kg of pretreated rice husk ash and dissolve it in 100L of anhydrous ethanol, add 10kg of amino silicone oil while stirring, react in a constant temperature water bath at 70°C for 8h, wash, filter and dry to obtain the preliminarily modified rice husk ash for use; S2, take 6kg polyphenylene sulfide and 0.1kg p-chlorobenzoic acid, 0.18kg sodium hydroxide, 25L 1-methyl-pyrrolidone, pass nitrogen protection, stir evenly at 350r / min, heat to 250℃ at a rate of 1℃ / min, keep warm for 3.5h, then cool to 220℃ at the same rate, keep warm for 20min, finally cool to 140℃ at the same rate, filter, wash with 0.1% acetic acid solution for several times and dry to obtain modified polyphenylene sulfide; S3, take 8 kg of modified polyphenylene sulfide and disperse it in 100 L of anhydrous toluene, add 10 kg of rice husk ash preliminarily modified in S1, then add 0.5 ml of acetic acid, react at 100 ° C for 10 hours, filter and wash, and Soxhlet extract with ethanol solution for 24 hours, vacuum dry to constant weight, and obtain modified rice husk ash.
[0036] (3) Take 10 kg of modified rice husk ash, 1 kg of vermiculite, 0.8 kg of methyl laurate, 9 kg of liquid paraffin and 90 kg of loess, mix them, sprinkle 22 kg of water while stirring, stir and mix evenly, seal and place for 24 hours, and obtain the modified loess.
[0037] Example 5 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 500° C. for 75 min, and then ground at 225 r / min for 30 min to obtain pretreated rice husk ash; (2) Modified rice husk ash: S1. Take 10 kg of calcined rice husk ash and dissolve it in 100 L of anhydrous ethanol, add 8 kg of amino silicone oil while stirring, react in a constant temperature water bath at 60° C. for 9 h, wash, filter and dry to obtain the initially modified rice husk ash for use; S2, take 6kg polyphenylene sulfide and 0.1kg p-chlorobenzoic acid, 0.18kg sodium hydroxide, 25L 1-methyl-pyrrolidone, pass nitrogen protection, stir evenly at 350r / min, heat to 220°C at a rate of 3°C / min, keep warm for 4h, then cool to 200°C at the same rate, keep warm for 30min, finally cool to 120°C at the same rate, filter, wash with 0.1% acetic acid solution for several times and dry to obtain modified polyphenylene sulfide; S3, taking 12 kg of modified polyphenylene sulfide and dispersing it in 100 L of anhydrous toluene, adding 10 kg of rice husk ash preliminarily modified in S1, and then adding 0.5 ml of acetic acid, reacting at 90 ° C for 12 hours, filtering, washing, and Soxhlet extraction with ethanol solution for 24 hours, vacuum drying to constant weight, to obtain modified rice husk ash; (3) Take 10 kg of modified rice husk ash, 1 kg of vermiculite, 0.8 kg of methyl laurate, 9 kg of liquid paraffin and 90 kg of loess, mix them, sprinkle 22 kg of water while stirring, stir and mix evenly, seal and place for 24 hours, and obtain the modified loess.
[0038] Example 6 A kind of improved loess, preparation comprises the following steps: (1) 15 kg of rice husk ash was calcined at 500° C. for 75 min, and then ground at 225 r / min for 30 min to obtain pretreated rice husk ash; (2) Modified rice husk ash: S1. Take 10 kg of calcined rice husk ash and dissolve it in 100 L of anhydrous ethanol. Add 12 kg of amino silicone oil while stirring. React in a constant temperature water bath at 90° C. for 9 h. After washing, filtering and drying, obtain the initially modified rice husk ash for use. S2, take 6kg polyphenylene sulfide and 0.1kg p-chlorobenzoic acid, 0.18kg sodium hydroxide, 25L 1-methyl-pyrrolidone, pass nitrogen protection, stir evenly at 350r / min, heat to 235°C at a rate of 2°C / min, keep warm for 3h, then cool to 210°C at the same rate, keep warm for 20min, finally cool to 130°C at the same rate, filter, wash with 0.1% acetic acid solution for several times and dry to obtain modified polyphenylene sulfide; S3. Take 10 kg of modified polyphenylene sulfide and disperse it in 100 L of anhydrous toluene, add 10 kg of rice husk ash preliminarily modified in S1, and then add 0.5 ml of acetic acid, react at 110 ° C for 11 hours, filter and wash, and Soxhlet extract with ethanol solution for 24 hours, vacuum dry to constant weight, and obtain modified rice husk ash.
[0039] (3) Take 10 kg of modified rice husk ash, 1 kg of vermiculite, 0.8 kg of methyl laurate, 9 kg of liquid paraffin and 90 kg of loess, mix them, sprinkle 22 kg of water while stirring, stir and mix evenly, seal and place for 24 hours, and obtain the modified loess.
[0040] Example 7 A modified loess, which is different from Example 1 in that the loess used in this example is dried at 100° C. to constant weight and then crushed through a 2 mm sieve, and the other steps are the same as Example 1.
[0041] The application is the same as in Example 1.
[0042] Example 8 A modified loess, which is different from Example 1 in that the loess used in this example is dried at 110° C. to constant weight and then crushed through a 5 mm sieve, and the other steps are the same as Example 1.
[0043] The application is the same as in Example 1.
[0044] Example 9 A modified loess, which is different from Example 1 in that this embodiment also includes 1 kg of calcium sulphoaluminate, and the preparation includes the following steps: (1) 15 kg of rice husk ash was calcined at 500° C. for 75 min, and then ground at 225 r / min for 30 min to obtain pretreated rice husk ash; (2) 10 kg of pretreated rice husk ash, 1 kg of vermiculite, 0.8 kg of methyl laurate, 9 kg of liquid paraffin, 1 kg of calcium sulfoaluminate and 90 kg of loess were mixed, and 22 kg of water was sprinkled into the mixture while stirring. After stirring and mixing evenly, the mixture was sealed and placed for 24 hours to obtain the improved loess.
[0045] The application is the same as in Example 1.
[0046] Example 10 A modified loess, which is different from Example 9 in that 3 kg of calcium sulfoaluminate is included in this example, and the other steps are the same as Example 1.
[0047] The application is the same as in Example 1.
[0048] Comparative Example Comparative Example 1 An improved loess, which is different from Example 1 in that in this comparative example, the rice husk ash is taken out after being calcined at 700° C. for 75 minutes, and ground at 225 r / min for 30 minutes, and the other steps are the same as Example 1; An application of improved loess, same as Example 1.
[0049] Comparative Example 2 An improved loess, which is different from Example 1 in that in this comparative example, the rice husk ash is taken out after being calcined at 400° C. for 75 minutes, and ground at 225 r / min for 30 minutes, and the other steps are the same as Example 1; An application of improved loess, same as Example 1.
[0050] Comparative Example 3 A modified loess, which is different from Example 1 in that rice husk ash is not added in this comparative example.
[0051] Comparative Example 4 A modified loess, which is different from Example 1 in that methyl laurate and liquid paraffin are not added in this comparative example.
[0052] Performance testing Detection method / test method The improved loess sample was prepared according to the two-end static pressure method. The sample size was 50×50×50mm. The sample was demoulded by a hydraulic demoulding machine. Then the sample was wrapped with plastic wrap and cured at room temperature for 1 day. Unconfined compressive strength test: According to GB / T 50123-2019 Geotechnical Test Method Standard, the compressive strength of the sample was tested. The cured sample was taken out, smeared with vaseline on both ends, and placed on the pressure plate. The compressive strength of the sample was tested using an electronic universal testing machine. The sample and the upper pressure plate were just in contact through computer control. Then the displacement and force readings were adjusted to zero. The test strain rate was set to 1 mm / min. After the specimen was damaged, the maximum value in the image was recorded as the maximum bearing capacity of the specimen. The damage form of the specimen was plastic failure. In order to reduce the test error, parallel tests were performed on each group of specimens and the average value was taken. The compressive strength was calculated using formula (1): F is the pressure value corresponding to the destruction of the sample, kN; A is the bottom area of the sample, mm2 ; P is the compressive strength value, MPa.
[0053] Unconfined compressive strength test of improved loess under freeze-thaw environment: The cured samples were tested after 3 and 7 freeze-thaw cycles in 20℃ and -20℃ environments, and the compressive strength of the improved loess after freeze-thaw cycles was calculated.
[0054] Table 1 Test results Combining Examples 1-3 and Comparative Examples 1-2 and Table 1, it can be seen that the experimental data of Examples 1-3 are better than those of Comparative Examples 1-2, indicating that the calcination temperature affects the modification effect of rice husk ash on loess. Pre-treating the rice husk ash and calcining it at 500-600°C helps to increase the content and activity of amorphous silica in the rice husk ash, which is beneficial to its subsequent modification operation on loess, while improving the internal soil structure, thereby improving the compressive strength and durability of the loess.
[0055] Combining Example 1 with Comparative Example 3 and Table 1, it can be seen that the various test data of Example 1 are better than those of Comparative Example 3, indicating that the addition of rice husk ash can change the microstructure of loess, reduce the distance between soil particles, make them more closely arranged, and enhance the integrity and stability of the soil.
[0056] Combining Example 1 with Comparative Example 4 and Table 1, it can be seen that the various test data of Example 1 are better than those of Comparative Example 4, indicating that the addition of methyl laurate and liquid paraffin can improve the pore structure and water retention capacity of loess by increasing the organic matter content of the soil, thereby improving the durability under freeze-thaw cycles. Among them, liquid paraffin can improve the compaction of loess and form a protective film, further improving its compressive strength and durability.
[0057] Combining Example 1 with Examples 4-6 and Table 1, it can be seen that the experimental data of Examples 4-6 are better than those of Example 1, indicating that modifying rice husk ash with polyphenylene sulfide and adding it to loess can further improve the ability of the improved loess to resist deformation and damage by external forces, and further improve the compressive strength of the improved loess.
[0058] Combining Example 1 with Examples 7-8 and Table 1, it can be seen that the test data of Examples 7-8 are slightly better than those of Example 1, indicating that by further refining the loess, its particle size distribution can be more uniform, and it can better contact and react with other modified components to improve the compressive strength and durability of the improved loess.
[0059] Combining Example 1 with Examples 9-10 and Table 1, it can be seen that the test data of Examples 9-10 are better than those of Example 1, indicating that the addition of calcium sulfoaluminate can further fill the pores between the loess particles, and at the same time, the hydrated calcium sulfoaluminate crystals can be interwoven with raw materials such as rice husk ash to form a more solid network structure, thereby improving the compressive strength of the soil.
[0060] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for improving loess using biomass ash, characterized in that: The steps include: (1) calcining the biomass ash at 500-600°C for 60-90 minutes, taking it out, and grinding it at 200-250 r / min for 30-40 minutes to obtain pretreated biomass ash; (2) Mix the pretreated biomass ash with vermiculite, methyl laurate, liquid paraffin and loess, sprinkle water while stirring, and after mixing evenly, seal and place for 18-24 hours to obtain improved loess; the biomass ash is rice husk ash.
2. The method for improving loess using biomass ash according to claim 1, characterized in that: In the improved loess raw material, the added amounts of each raw material are as follows: 80-100 parts of loess, 8-10 parts of rice husk ash, 8-10 parts of liquid paraffin, 0.5-0.8 parts of methyl laurate, 1-2 parts of vermiculite and 20-25 parts of water.
3. The method for improving loess using biomass ash according to claim 2, characterized in that: The loess is dried at 100-110° C. to constant weight, crushed and passed through a 2-5 mm sieve.
4. The method for improving loess using biomass ash according to claim 1, characterized in that: The rice husk ash is further subjected to a modification operation after the pretreatment operation, and the modification steps are as follows: S1. Dissolve the calcined rice husk ash in anhydrous ethanol, add amino silicone oil while stirring, react in a constant temperature water bath at 60-90° C. for 8-9 hours, wash, filter, and dry to obtain preliminarily modified rice husk ash for later use; S2, take polyphenylene sulfide and p-chlorobenzoic acid, sodium hydroxide, 1-methyl-pyrrolidone, pass nitrogen protection, stir evenly, heat to 220-250°C at a rate of 1-3°C / min, keep warm for 3-4h, then cool to 200-220°C at the same rate, keep warm for 20-30min, and finally cool to 120-140°C at the same rate, filter, wash and dry to obtain modified polyphenylene sulfide; S3. Disperse the modified polyphenylene sulfide in anhydrous toluene, add the rice husk ash preliminarily modified in S1, and then add acetic acid, react at 90-110°C for 10-12h, filter, wash, and extract with ethanol solution for 24h, and vacuum dry to constant weight to obtain modified rice husk ash.
5. The method for improving loess using biomass ash according to claim 4, characterized in that: The weight ratio of rice husk ash to amino silicone oil in S1 is 1:2.8-4.
2.
6. The method for improving loess using biomass ash according to claim 4, characterized in that: The weight ratio of modified polyphenylene sulfide to preliminarily modified rice husk ash in S3 is 1:0.8-1.
2.
7. The method for improving loess using biomass ash according to claim 2, characterized in that: The raw materials also include 1-3 parts of calcium sulphoaluminate.
8. Use of improved loess prepared according to any one of claims 1 to 7 in engineering fillers.