Method for preparing mesophase pitch from medium and low temperature coal tar pitch

Through the refining, hydrogenation and polycondensation steps of medium and low temperature coal tar asphalt, the problem of failure to develop the preparation of mesophase asphalt from coal tar asphalt in China has been solved, and the preparation of mesophase asphalt with high content and high performance has been achieved, reducing costs and Improved product performance.

CN118956435APending Publication Date: 2024-11-15XI'AN PETROLEUM UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410923386.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The technology for preparing mesophase asphalt using coal tar asphalt as raw material has not yet been developed in China, which has led to a gap in the performance of carbon fiber products compared with that of Japan and the United States, limiting the development and industrialization of my country's carbon fiber technology.

Method used

Through the refining, hydrogenation and polycondensation steps of medium and low temperature coal tar asphalt, the mesophase asphalt with an intermediate phase content of up to 99% was successfully produced, including step 1: using medium and low temperature pyrolysis coal tar asphalt as raw material, add solvent and heat and stir, Filtration and distillation to obtain refined asphalt; Step 2: Hydrotate is hydrotreated; Step 3: Polycondensation reaction is carried out at a pressure of 300°C and 2Mpa to obtain the final mesophase asphalt.

Benefits of technology

The preparation cost is reduced, the softening point and mesophase content of mesophase asphalt are increased, which is significantly better than the performance of existing products, and the preparation of low-cost and high-quality spunable asphalt is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956435A_ABST
    Figure CN118956435A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing mesophase pitch from medium and low temperature coal tar pitch. Comprising the following steps: step 1, adding a solvent into medium-low temperature pyrolysis coal tar pitch serving as a raw material, mixing, heating, stirring, filtering and distilling to obtain refined pitch; step 2, adding the refined asphalt into a solvent for hydrotreating to obtain hydrofined asphalt; and step 3, carrying out condensation polymerization on the hydrofined pitch at 300 DEG C under the pressure of 2Mpa to obtain the final mesophase pitch. The mesophase pitch with the mesophase content up to 99% is successfully produced by taking the medium and low temperature coal tar pitch as a raw material through the steps of refining, hydrogenation, polycondensation and the like, so that the existing technical problems of preparing the mesophase pitch from the coal tar pitch in China at present are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation methods of mesophase asphalt, and in particular to a method for preparing mesophase asphalt from medium- and low-temperature coal tar asphalt. Background Art

[0002] Carbon fiber is a fibrous high-strength carbon material with excellent properties such as high strength, high modulus, high thermal conductivity, and high temperature resistance. It is not only an indispensable engineering material in the technical fields of aerospace and national defense, but also a key material widely used in new energy vehicles, medical equipment, sports goods and other fields. It belongs to the country's high-tech special fiber for military and civilian use. According to the different raw materials, carbon fiber can be classified into polyacrylonitrile (PAN)-based carbon fiber, asphalt-based carbon fiber and viscose-based carbon fiber. Among them, asphalt-based carbon fiber is prepared with asphalt as raw material. It not only has the characteristics of a wide range of raw material sources, high carbonization yield, and easy graphitization, but also has high modulus and high thermal conductivity that are difficult to achieve with the other two types of carbon fibers, which makes asphalt-based carbon fiber have broad application prospects in the defense and civilian fields.

[0003] The preparation of high-end carbon-based new materials with coal tar pitch is a cutting-edge field of materials science in the international energy industry. It has a wide range of uses in the military and civilian fields and has attracted much attention from all countries. Among them, a small number of companies in the United States and Japan use oil-based or coal-based two different raw materials to prepare mesophase pitch, which is at the international leading level. The research on asphalt-based carbon fiber can be traced back to the late 1950s. It was successfully developed by Professor Otani Shanlang of Gunma University in Japan in the early 1960s, and industrialized production was achieved in Kureha Chemical Company in Japan in the late 1960s. In 1975, Union Carbide Corporation (UCC) of the United States began to develop high-performance mesophase carbon fiber "Thomel-P55" and achieved success, marking the maturity of the manufacturing process of asphalt-based carbon fiber. The company officially put into production mesophase pitch in 1980. Mitsubishi Chemical Corporation of Japan is one of the first companies in the world to develop asphalt-based carbon fiber, and built an industrial demonstration device of 500 tons / year of mesophase pitch carbon fiber in 1987, marking the entry of asphalt-based carbon fiber into the fast lane of industrial development.

[0004] At present, the production of mesophase pitch carbon fiber is monopolized by three companies, namely: Mitsubishi Chemical Corporation of Japan, which uses naphthalene asphalt and coal-based asphalt as raw materials, and the mesophase asphalt production capacity is about 1,200t / a; Japan Graphite Fiber Company, which uses coal-based asphalt as raw material, and the mesophase asphalt production capacity is about 230t / a; American Cytec Engineering Materials Company, which uses petroleum-based asphalt as raw material, and the mesophase asphalt production capacity is about 400t / a. However, affected by the confidentiality of foreign technology, the carbon fiber products of the above three companies are not sold domestically. However, at present, domestic manufacturers all use petroleum asphalt as raw material to produce mesophase pitch carbon fiber, and have not developed the technology of preparing mesophase pitch carbon fiber with coal tar asphalt as raw material. And due to process and technical reasons, there is still a certain gap between the product performance and that of developed countries such as Japan and the United States. It belongs to undeveloped materials, which seriously restricts the development of related fields such as defense in China. Breaking through the monopoly of Japan and the United States on carbon fiber core technology and doing a good job in large-scale industrialization of mesophase pitch-based carbon fiber is in line with my country's current strategic layout.

[0005] The structure of mesophase asphalt determines its processing performance and the quality of carbon fiber products. Although my country has mastered some asphalt synthesis technologies, most of them use petroleum-based substances as raw materials. Therefore, the preparation of low-cost and high-quality spinnable asphalt is still a bottleneck for the development of carbon fiber technology in my country. Breaking through the theoretical basis and technical problems of coal-based asphalt raw materials is an urgent problem to be solved. Against the background of my country's increasing dependence on foreign oil resources, it is crucial to give full play to the advantages of my country's coal resources and use my country's huge medium and low-temperature coal tar asphalt as raw materials to produce low-cost, high-quality spinnable mesophase asphalt. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing mesophase asphalt from medium-low temperature coal tar pitch. The present invention uses medium-low temperature coal tar pitch as raw material, and through refining, polycondensation and other steps, successfully produces mesophase asphalt with a mesophase content of up to 99%, solving the existing technical problems of preparing mesophase asphalt from coal tar pitch in China.

[0007] The present invention is achieved through the following technical solutions:

[0008] The present invention relates to a method for preparing mesophase pitch from medium- and low-temperature coal tar pitch, comprising the following steps:

[0009] Step 1, refining: using medium-low temperature pyrolysis coal tar pitch as raw material, adding solvent and mixing, heating and stirring, filtering, and distilling to obtain refined pitch;

[0010] Step 2, hydrogenation: adding a solvent to the refined asphalt for hydrogenation treatment to change the molecular structure of the refined asphalt to obtain hydrogenated refined asphalt;

[0011] Step 3, polycondensation: subjecting the hydrogenated refined asphalt to a polycondensation reaction at 300°C and a pressure of 2 MPa to obtain the final mesophase asphalt.

[0012] Preferably, in step 1, the softening point of the medium-low temperature pyrolysis coal tar pitch is 80° C.; the toluene insoluble matter of the medium-low temperature pyrolysis coal tar pitch is 3-5%, and the quinoline insoluble matter content is 0.5-1%.

[0013] Preferably, in step 1, the solvent is one or a mixture of wash oil, kerosene, naphthalene oil, gasoline, diesel, and tetrahydrofuran.

[0014] Preferably, the solvent is a mixture of two of washing oil, kerosene, naphthalene oil, gasoline, diesel and tetrahydrofuran, and the mass ratio of the mixture is 1:1.

[0015] Preferably, in step 1, the temperature of the heating and stirring is 150-350°C, the filtration is hot filtration at 40-150°C, and the distillation method is reduced pressure distillation at 200-350°C.

[0016] Preferably, in step 2, the solvent is one or a mixture of hydrogen peroxide, ethanol, tetralin, decalin, and tetrahydrofuran.

[0017] Preferably, the solvent is a mixture of two of hydrogen peroxide, ethanol, tetralin, decalin, and tetrahydrofuran, and the mass ratio of the mixture is 1:1.

[0018] Preferably, in step 3, the polycondensation reaction time is 4 to 10 hours.

[0019] Preferably, in step 3, the mesophase content of the final mesophase asphalt is 80-99%.

[0020] Preferably, in step 3, the softening point of the final mesophase asphalt is 270-290°C.

[0021] The present invention has the following advantages:

[0022] (1) Compared with the prior art, the present invention uses medium-low temperature coal tar as raw material, and after hydrogenation refining of the whole fraction (requiring the use of a catalyst), cuts the heavy fraction and performs secondary hydrogenation, and finally performs polycondensation to prepare the intermediate phase asphalt; while the raw material of the present invention is medium-low temperature coal tar asphalt, which is an industrial product with low cost and is cheap and easy to obtain; there is no catalytic hydrogenation refining section in the preparation process, which reduces the steps of the section and reduces the preparation cost.

[0023] (2) Compared with the prior art, the softening point of the mesophase asphalt obtained by the prior art method is 245-265°C, and the quinoline insoluble matter in the mesophase asphalt is less than 30%; while the softening point of the mesophase asphalt prepared by the method involved in the present invention is 270-290°C, and the mesophase content is as high as 99%, which is much better than the performance of the existing products. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a polarizing microscope image of the mesophase pitch prepared by the method of the present invention in Example 1 of the present invention;

[0025] Figure 2 is a polarizing microscope image of the mesophase pitch prepared by the method of the present invention in Example 2 of the present invention;

[0026] Figure 3 is a polarizing microscope image of the mesophase pitch prepared by the method of the present invention in Example 3 of the present invention;

[0027] Figure 4 This is a polarizing microscope image of the mesophase pitch prepared by the method of Comparative Example 1;

[0028] Figure 5 This is a polarizing microscope image of the mesophase pitch prepared by the method of Comparative Example 2;

[0029] Figure 6 This is a polarizing microscope image of the mesophase pitch prepared by the method of Comparative Example 3;

[0030] Figure 7 It is the roadmap of the present invention;

[0031] Figure 8 It is a preparation process diagram of the refining process involved in the present invention. DETAILED DESCRIPTION

[0032] The present invention is described in detail below in conjunction with specific embodiments. It should be noted that the following embodiments are only further descriptions of the present invention, but the protection scope of the present invention is not limited to the following embodiments.

[0033] Example 1

[0034] This embodiment relates to a method for preparing mesophase pitch from medium- and low-temperature coal tar pitch. Figure 7 As shown, including:

[0035] Step 1, select medium and low temperature coal tar pitch as raw material, use tetrahydrofuran and washing oil mixed in a ratio of 1:1 as solvent, purify the pitch at 300°C, perform hot filtration at 100°C, perform vacuum distillation at 300°C to remove the solvent, and obtain refined pitch, see Figure 8 As shown;

[0036] Step 2, using a mixed solvent of tetralin and decalin (1:1) as a hydrogen supply solvent, hydrogenating at 350° C. and a pressure of 1 MPa for 2 hours to obtain a hydrorefined asphalt;

[0037] Step 3, polycondensation is carried out at 300°C and 2 MPa for 10 h to obtain an asphalt product with a mesophase content of 81%, such as Figure 1 As shown, it can be seen that the sample has obvious wide-area flow lines, proving that the material has a high content of intermediate phase.

[0038] The raw material involved in this embodiment is medium-low temperature pyrolysis coal tar pitch in northern Shaanxi. The softening point of the medium-temperature coal tar pitch is 80° C., the toluene insoluble matter of the raw material asphalt is 3-5%, and the quinoline insoluble matter content is 0.5-1%.

[0039] Example 2

[0040] This embodiment relates to a method for preparing mesophase pitch from medium- and low-temperature coal tar pitch, comprising:

[0041] Step 1, selecting medium-low temperature coal tar pitch as raw material, using wash oil as solvent, purifying the pitch at 320° C., performing hot filtration at 110° C., and performing reduced pressure distillation at 320° C. to remove the solvent, to obtain refined asphalt;

[0042] Step 2, using a mixed solvent of tetralin and decalin (1:1) as a hydrogen supply solvent, hydrogenating at 350° C. and a pressure of 3 MPa for 4 hours to obtain a hydrorefined asphalt;

[0043] Step 3, polycondensation is carried out at 300°C and 0.2 MPa for 10 h to obtain an asphalt product with a mesophase content of up to 91%, see Figure 2 As shown, it can be seen that the sample has an obvious wide-area flow line, proving that the material has a high content of intermediate phase.

[0044] The raw material involved in this embodiment is medium-low temperature pyrolysis coal tar pitch in northern Shaanxi. The softening point of the medium-temperature coal tar pitch is 80° C., the toluene insoluble matter of the raw material asphalt is 3-5%, and the quinoline insoluble matter content is 0.5-1%.

[0045] Example 3

[0046] This embodiment relates to a method for preparing mesophase pitch from medium- and low-temperature coal tar pitch, comprising:

[0047] Step 1, selecting medium and low temperature coal tar pitch as raw material, using kerosene and washing oil mixed in a ratio of 1:1 as solvent, purifying the pitch at 310°C, performing hot filtration at 80°C, and performing reduced pressure distillation at 320°C to remove the solvent, to obtain refined asphalt;

[0048] Step 2, using a mixed solvent of tetralin and decalin (1:1) as a hydrogen supply solvent, hydrogenating at 400° C. and a pressure of 4 MPa for 5 hours to obtain a hydrorefined asphalt;

[0049] Step 3, polycondensation is carried out at 420°C and 0 MPa for 12 h to obtain an asphalt product with a mesophase content of up to 99%, see Figure 3 As shown, it can be seen that the sample has an obvious wide-area flow line, proving that the material has a high content of intermediate phase.

[0050] The raw material involved in this embodiment is medium-low temperature pyrolysis coal tar pitch in northern Shaanxi. The softening point of the medium-temperature coal tar pitch is 80° C., the toluene insoluble matter of the raw material asphalt is 3-5%, and the quinoline insoluble matter content is 0.5-1%.

[0051] Comparative Example 1

[0052] The raw materials were the same as those in Examples 1 to 3. The raw materials were not refined. Instead, a mixed solvent of tetralin and decalin (1:1) was directly used as a hydrogen supply solvent. Hydrogenation was performed at 350°C and a pressure of 1 MPa for 2 h to obtain a hydrogenated refined asphalt. Polycondensation was performed at 300°C and a pressure of 2 MPa for 10 h to obtain a product in which there was substantially no mesophase asphalt. Figure 4 As shown, it can be seen that the sample does not have wide-area streamlines, that is, there is no mesophase asphalt.

[0053] Comparative Example 2

[0054] Select medium and low temperature coal tar pitch as raw material, use tetrahydrofuran and washing oil as mixed solvent, purify the pitch at 300℃, perform hot filtration at 100℃, and remove the solvent by vacuum distillation at 300℃ to obtain refined asphalt. Without hydrogenation, directly carry out polycondensation at 300℃ and 0.5Mpa pressure for 10h, and the obtained product basically does not contain mesophase asphalt, see Figure 5 As shown, it can be seen that the sample does not have wide-area streamlines, that is, there is no mesophase asphalt.

[0055] Comparative Example 3

[0056] Select medium and low temperature coal tar pitch as raw material, use tetrahydrofuran and washing oil as mixed solvent, purify the pitch at 300℃, perform hot filtration at 100℃, and remove the solvent by vacuum distillation at 300℃ to obtain refined asphalt. Without hydrogenation, directly carry out polycondensation at 300℃ and 0.5Mpa pressure for 10h, and the obtained product basically does not contain mesophase asphalt, see Figure 6 As shown, it can be seen that the sample does not have wide-area streamlines, that is, there is no mesophase asphalt.

[0057] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which will not affect the essence of the present invention.

Claims

1. A method for preparing mesophase pitch from medium- and low-temperature coal tar pitch, characterized in that: The following steps are involved: Step 1, refining: using medium-low temperature pyrolysis coal tar pitch as raw material, adding solvent and mixing, heating and stirring, filtering, and distilling to obtain refined pitch; Step 2, hydrogenation: adding a solvent to the refined asphalt for hydrogenation treatment to obtain hydrogenated refined asphalt; Step 3, polycondensation: subjecting the hydrogenated refined asphalt to a polycondensation reaction at 300°C and a pressure of 2 MPa to obtain the final mesophase asphalt.

2. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 1, the softening point of the medium-low temperature pyrolysis coal tar pitch is 80° C.; the toluene insoluble matter content of the medium-low temperature pyrolysis coal tar pitch is 3-5%, and the quinoline insoluble matter content is 0.5-1%.

3. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 1, the solvent is one or a mixture of wash oil, kerosene, naphthalene oil, gasoline, diesel, and tetrahydrofuran.

4. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 3, characterized in that: The solvent is a mixture of two of washing oil, kerosene, naphthalene oil, gasoline, diesel and tetrahydrofuran, and the mixture of the two is in a mass ratio of 1:

1.

5. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 1, the temperature of the heating and stirring is 150-350° C., the filtration is hot filtration at 40-150° C., and the distillation method is reduced pressure distillation at 200-350° C.

6. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 2, the solvent is one or a mixture of hydrogen peroxide, ethanol, tetralin, decalin, and tetrahydrofuran.

7. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 6, characterized in that: The solvent is a mixture of two of hydrogen peroxide, ethanol, tetralin, decalin and tetrahydrofuran, and the mass ratio of the mixture is 1:

1.

8. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 3, the polycondensation reaction time is 4 to 10 hours.

9. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 3, the mesophase content of the final mesophase asphalt is 80-99%.

10. The method for preparing mesophase pitch from medium- and low-temperature coal tar pitch according to claim 1, characterized in that: In step 3, the softening point of the final mesophase asphalt is 270-290°C.

Citation Information

Cited By

  • Coal-series mesophase pitch and preparation method thereof

    CN122104264A