Method for smelting all-vanadium titano-magnetite pellets through all-oxygen-carbon cycle blast furnace

Through the all-oxygen carbon cycle blast furnace process and the application of all-vana titanium magnetite pellets, the problem of titanium oxide over-reduction in vanadium titanium magnetite smelting is solved, efficient titanium recycling and low-carbon smelting are achieved, and solids are reduced Fuel consumption and carbon emissions have improved smelting efficiency and concentrate utilization.

CN118957188APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411166866.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing blast furnace smelting process is difficult to effectively deal with the problem of overreduction of titanium oxide in vanadium titanium magnetite, which leads to the viscosity of slag, foam slag and slag iron, and the difficulty in recycling of titanium, which limits the smelting of vanadium titanium pellets in blast furnace. Application in.

Method used

The fully oxygen carbon cycle blast furnace process is adopted, pure oxygen is blown into the blast furnace air outlet, and the furnace top gas is processed using the carbon dioxide separation and capture unit. The heating gas is blown into the segments, and the process parameters, furnace material composition, fabric system, and air supply system are adjusted. And the operating system, all-vana titanium magnetite pellets are used as furnace charges to increase the titanium dioxide content and titanium recovery rate of the slag.

Benefits of technology

It significantly reduces solid fuel consumption and carbon emission intensity, inhibits the generation of solid titanium carbonitride solution, increases the titanium content in the slag, realizes efficient smelting and titanium recovery of vanadium titanium magnetite, and reduces smelting costs and carbon emissions. Improved yield and concentrate usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957188A_ABST
    Figure CN118957188A_ABST
Patent Text Reader

Abstract

The method comprises the steps that pure oxygen is blown in through a blast furnace tuyere, after blast furnace top gas passes through a carbon dioxide separation and capture unit, one part of the gas enters a gas pipe network, and the other part of the gas is sent to a hot blast stove to be heated; the heated coal gas is blown into the blast furnace through a hearth tuyere and a furnace body tuyere respectively; determining process parameters, furnace charge components, a material distribution system, an air supply system, a slagging system, a heat system and an operation system; and carrying out blast furnace smelting by adopting furnace charge comprising all-vanadium titano-magnetite pellets. By means of the method, the solid fuel consumption and the carbon emission intensity of an existing blast furnace vanadium titano-magnetite smelting process can be remarkably reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metallurgy, and more specifically to a method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace. Background Art

[0002] The steel industry is a pillar industry of my country's economy and one of the main contributors to industrial carbon emissions. With the tightening of emission policies, the development and industrial promotion of low-carbon smelting technology has become imperative. Blast furnace smelting is the current mainstream ironmaking process. Continuing to upgrade and transform the smelting process around blast furnaces is a relatively stable and quickly implemented low-carbon technical solution in the short term; such as top gas (carbon) circulation, hydrogen-containing gas injection, oxygen blast furnace and other technical solutions, or a combination of various solutions, can theoretically achieve significant carbon emission reductions.

[0003] The oxygen blast furnace process refers to a smelting technology that uses an ultra-high oxygen-enriched or pure oxygen atmosphere to replace the hot blast (i.e., hot air) in a traditional blast furnace. It is generally necessary to cooperate with the top gas (carbon) circulation process to achieve the purpose of carbon reduction. The so-called top gas circulation or carbon circulation process is actually to separate and capture carbon dioxide (CO2) in the top gas, and to recycle the separated reducing components such as carbon monoxide (CO) and hydrogen (H2). The main purpose of using full oxygen is to reduce the nitrogen (N2) content in the top gas to facilitate separation from carbon dioxide; at the same time, the full oxygen atmosphere can significantly increase the reduction potential in the furnace gas, promote the development of indirect reduction, and reduce direct reduction carbon consumption. Many laboratory basic theoretical studies and numerical simulation studies have shown that the full oxygen carbon cycle process can significantly reduce fuel consumption, increase yield and significantly reduce carbon emissions.

[0004] On the other hand, the current blast furnace charge structure is mostly based on sintered ore, with an average charge ratio of more than 70%. However, the sintering process has high energy consumption and large emissions of flue gas and pollutants; in comparison, the energy consumption and pollutant emissions of the pelletizing process are only less than 50% of the sintering process, and carbon dioxide emissions are about 30% of sintering. It can be seen that increasing the proportion of pellets used in blast furnace ironmaking is conducive to reducing pollutants and carbon emissions in the ironmaking system. In addition, pellets themselves have the characteristics of high grade and low slag ratio, so the smelting of a large proportion of pellets (50%) can also play a role in energy saving and consumption reduction. Based on this, the industry has gradually reached a consensus on increasing the proportion of pellets entering the furnace.

[0005] However, most of the above studies are limited to ordinary iron ore, while there are relatively few studies based on vanadium-titanium magnetite smelting. my country's Panxi region has rich reserves of vanadium-titanium magnetite resources, which are important strategic resources in my country. After years of hard work, my country has successfully developed a vanadium-titanium magnetite smelting process based on the blast furnace-converter process. However, the existing process cannot achieve long-term full-vanadium-titanium magnetite smelting. The main reason is that the titanium oxide in vanadium-titanium magnetite is easily over-reduced to high-melting-point substances, such as titanium carbide (TiC), titanium nitride (TiN) and titanium carbonitride solid solution (Ti(C,N)), resulting in slag viscosity, foamy slag, difficulty in iron discharge and difficulty in separating slag and iron. The charge structure of an ordinary blast furnace is generally 70% sintered ore and 30% pelletized ore. These charge structures are mainly based on ordinary iron concentrate (Fe2O3). When the charge is mainly vanadium-titanium magnetite ((Fe2O3)x·(TiO2)y), increasing the proportion of vanadium-titanium pellets will lead to the enrichment of titanium dioxide (TiO2) in the slag, which will cause a series of problems in blast furnace operation. Therefore, it is generally necessary to add some ordinary ore to the charge structure to dilute the titanium dioxide content in the slag, but this also makes it difficult to recover titanium (Ti) in the slag.

[0006] Based on this, there is room for improvement in the smelting problem of all-vanadium-titanium pellets entering the vanadium-titanium blast furnace. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide a method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace to solve the technical problem of smelting all-vanadium titanium pellets into a vanadium-titanium blast furnace.

[0008] In order to achieve the above object, the technical solution provided by the present invention is: A method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace comprises: blowing pure oxygen into the blast furnace tuyere, a portion of the blast furnace top gas enters the gas pipe network after passing through a carbon dioxide separation and capture unit, and the other portion is sent to a hot blast furnace for heating, and the heated gas is blown into the blast furnace through the furnace cylinder tuyere and the furnace body tuyere respectively; determining process parameters, charge composition, charge distribution system, air supply system, slag making system, thermal system and operation system; and using a charge including all-vanadium titanium magnetite pellets for blast furnace smelting.

[0009] In some embodiments, determining the process parameters includes: performing mass and energy balance calculations on the unit including the furnace belly + furnace hearth, furnace body and hot blast furnace, and determining the process parameters by adjusting parameters including the air supply volume of the hot blast furnace, the process parameters including parameters in the material distribution system, air supply system and heat system.

[0010] In some embodiments, determining the charge composition includes: using all-vanadium titanium magnetite pellets into the furnace, and additionally adding alkaline components to cause the all-vanadium titanium magnetite pellets to change from acidic to alkaline, wherein the preparation requirements of the all-vanadium titanium magnetite pellets include average particle size, compressive strength, roasting conditions, reduction expansion index, medium-temperature reduction degree, softening temperature, pressure difference steep rise temperature, and dripping temperature requirements.

[0011] In some embodiments, determining the charge distribution system includes: determining a maximum charge distribution angle and a minimum charge distribution angle and a charge batch weight, wherein the charge batch weight includes an ore batch weight and a coke batch weight.

[0012] In some embodiments, determining the air supply system includes: solving the air supply system based on local heat and mass balance, calculating the oxygen blowing amount, the furnace tuyere blowing amount, the furnace body blowing amount, the furnace belly gas amount, the furnace cylinder tuyere theoretical combustion temperature, the furnace body gas amount, the gas amount entering the hot blast furnace, the furnace top gas composition, the gas composition entering the hot blast furnace, and pure oxygen blowing in at room temperature without passing through the hot blast furnace.

[0013] In some embodiments, determining the slag making system includes: using self-fluxing all-vanadium titanium magnetite pellets to adjust the binary basicity, ternary basicity, calcium oxide content, titanium dioxide content, vanadium pentoxide content, magnesium-aluminum ratio, and slag amount of the slag.

[0014] In some embodiments, determining the thermal regime includes: determining the temperature of the molten iron, and determining the vanadium content, titanium content, silicon content, and sulfur content in the molten iron.

[0015] In some embodiments, determining the operating system includes: determining the material rate according to the blast furnace type selection and batch weight, determining the fuel ratio, the temperature of the heated gas, and determining the wind pressure, wind speed, blast kinetic energy, furnace top pressure, furnace top gas temperature, and setting up a waste heat recovery device on the blast furnace top.

[0016] In some embodiments, the oxygen injection rate is 220-250 Nm 3 / tHM, furnace tuyere injection volume is 1100~1300Nm 3 / tHM, furnace body injection volume is 600~700Nm 3 / tHM, the amount of gas in the furnace is 1500~1800Nm 3 / tHM, the theoretical combustion temperature of the furnace tuyere is 2000~2200℃, and the gas volume of the furnace is 2000~2500Nm 3 / tHM, the gas volume entering the hot blast furnace is 1700~1900 Nm 3 / tHM.

[0017] In some embodiments, the binary basicity of the slag is adjusted to 1.3-1.5, the ternary basicity is adjusted to 1.5-1.7, the calcium oxide content is adjusted to 23-28%, the titanium dioxide content is adjusted to 35-40%, the vanadium pentoxide content is adjusted to 0.2-1.0%, the magnesium-aluminum ratio is adjusted to 0.5-0.9, and the slag amount is adjusted to 450-480 kg / tHM.

[0018] The beneficial effects of the present invention are: The method of smelting all-vanadium-titanium magnetite pellets in a full oxygen-carbon cycle blast furnace of the present invention can significantly reduce the solid fuel consumption and carbon emission intensity of the existing blast furnace smelting process of vanadium-titanium magnetite. By injecting all oxygen, the oxygen potential is increased to inhibit the formation of titanium carbonitride solid solution, creating favorable conditions for the smooth operation of the furnace. At the same time, the use of all-vanadium-titanium magnetite pellets into the furnace has great cost and environmental advantages, further increasing the titanium content in the slag, and laying the necessary foundation for subsequent slag titanium extraction. The technology of smelting high-titanium vanadium-titanium magnetite in a full oxygen-carbon cycle blast furnace formed by the method of the present invention can be applied to all vanadium-titanium ore smelting enterprises, which can improve the blast furnace smelting yield of vanadium-titanium ore, reduce costs, and reduce the carbon reduction level of long-process smelting, and has extremely high economic and social value. The implementation of the method of the present invention is expected to reduce carbon by 20%, reduce the solid-fuel ratio by 30%, and increase the yield by 10%. At the same time, the utilization rate of vanadium-titanium magnetite concentrate can reach 100%, greatly reducing the dependence on high-grade ore. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.

[0020] Figure 1 It is a process schematic diagram corresponding to the method of smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace of the present invention; Figure 2 It is a schematic diagram of an embodiment of the method for smelting all-vanadium titanium magnetite pellets in a blast furnace with full oxygen-carbon cycle according to the present invention. DETAILED DESCRIPTION

[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0022] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.

[0023] The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace provided by the present invention adopts a full oxygen-carbon cycle blast furnace process to smelt all-vanadium titanium magnetite pellets. The corresponding process is as follows Figure 1 As shown: pure oxygen is blown into the tuyere, while hot air is blown into the tuyere of a conventional blast furnace; after the top gas passes through the carbon dioxide separation and capture unit, part of it enters the gas pipeline network, and part of it is sent to the hot blast furnace for heating. The heated gas is divided into two parts, one part is blown into the blast furnace through the furnace tuyere, and the other part is blown into the blast furnace through the furnace body tuyere. Among them, the main reason for a part of the gas to enter the gas pipeline network is to avoid nitrogen accumulation in the system; and the reason for dividing the heated gas into two streams and blowing them separately is to curb the "cooling on top and hot on the bottom" phenomenon caused by the increase in yield, and to directly heat the upper furnace charge with a part of the heated gas. In order to avoid nitrogen accumulation, a part of the gas after the removal of carbon dioxide is released through the gas pipeline network. The main component of this part of the gas is the same as the gas sent to the hot blast furnace for heating.

[0024] All-oxygen blasting greatly reduces the nitrogen in the reducing gas and increases the oxygen potential in the furnace, thus inhibiting the formation of high-melting-point substances such as titanium carbonitride solid solution, fundamentally solving the problem of high-vanadium titanium ore charge ratio smelting. At the same time, the all-oxygen blast furnace also reduces the difficulty of separating carbon dioxide from the top gas. In addition, the ultra-high reduction potential brought by the all-oxygen blast furnace is also conducive to reducing solid fuel consumption.

[0025] The CO2 separation and capture unit uses chemical absorption to separate CO2 from the top gas. The separated CO2 can be used as a chemical raw material or stored through mineralization. From the perspective of net carbon emissions, the top gas carbon cycle can achieve ultra-low emissions. The purified gas including carbon monoxide and hydrogen is injected into the blast furnace through the blast furnace hearth and can be used to replace part of the coal powder or coke consumption.

[0026] Since the heated coal gas is blown in stages, with the upper furnace body tuyere as the boundary, the blast furnace can be regarded as a combination of the upper "reduction section" and the lower "melting section". The "reduction section" is responsible for the pre-reduction of iron ore, while the "melting section" is responsible for the deep reduction of iron ore and the slag iron melting. The gas-solid ratio of the "reduction section" and the "melting section" is different. The gas volume of the "reduction section" is the sum of the belly gas volume and the furnace body injection gas volume. The working temperature of the hot blast furnace is generally 1150℃±10℃, and the ore softening temperature is generally 1200℃±10℃. Therefore, the blowing position of the upper furnace body tuyere needs to be above the soft melting zone to maximize heat utilization. Pure oxygen is blown in at room temperature without being heated by the hot blast furnace.

[0027] The problem of "cold on the top and hot on the bottom" in the blast furnace is avoided by injecting the heated gas in stages. Only part of the heated gas is used for injection at the tuyere of the blast furnace hearth to avoid excessive gas volume in the furnace belly causing liquid flooding and affecting smooth operation; at the same time, the remaining heated gas is used for injection at the tuyere of the blast furnace body, which increases the heat input intensity of the upper part of the furnace body and greatly improves the reduction potential of the furnace body.

[0028] The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace provided by the present invention comprises: using a blast furnace tuyere to blow pure oxygen, after the blast furnace top gas passes through a carbon dioxide separation and capture unit, a part of it enters a gas pipe network, and the other part is sent to a hot blast furnace for heating, and the heated gas is respectively blown into the blast furnace through a furnace cylinder tuyere and a furnace body tuyere; determining process parameters, charge composition, charge distribution system, air supply system, slag making system, thermal system and operation system; using a charge including all-vanadium titanium magnetite pellets to carry out blast furnace smelting.

[0029] Compared with the existing blast furnace operation, the method of smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace of the present invention adjusts the blast furnace smelting process, introduces top gas circulation and all-oxygen blast furnace operation to strengthen smelting and reduce carbon emissions; by adjusting the process parameters, material distribution system, air supply system, slag making system, etc., it is beneficial to the smooth operation of the furnace and improves the titanium content in the slag, solving the smelting problem of all-vanadium titanium pellets entering the vanadium-titanium blast furnace.

[0030] Under the conditions of vanadium-titanium magnetite pellet smelting, in order to ensure full reduction of the "reduction stage" and alleviate the lack of heat in the upper part, the gas volume in the furnace should be maintained at 2000-2500Nm 3 / tHM (cubic meters per ton of iron). In order to ensure the smooth operation of the blast furnace and the rapid slag and iron tapping, the temperature and volume of the tuyere and bosh gas need to reach a certain level to meet the gas-solid heat exchange requirements. However, the air volume per ton of iron should not be too high. Too high a blast volume requires greater blast kinetic energy and is prone to flooding, affecting air permeability. Therefore, it is considered to maintain the tuyere and bosh gas volume near the existing blast furnace indicators, that is, 1500~1800Nm 3 / tHM. At the same time, the theoretical combustion temperature should be maintained at 2000-2200℃.

[0031] In some embodiments, determining the process parameters includes: performing mass and energy balance calculations on the unit including the furnace belly + furnace hearth, furnace body and hot blast furnace, and determining the process parameters by adjusting parameters including the air supply volume of the hot blast furnace. The process parameters include parameters in the material distribution system, air supply system and heat system.

[0032] In some embodiments, determining the charge composition includes: using all-vanadium titanium magnetite pellets into the furnace, and additionally adding alkaline components to cause the all-vanadium titanium magnetite pellets to change from acidic to alkaline, wherein the preparation requirements of the all-vanadium titanium magnetite pellets include average particle size, compressive strength, roasting conditions, reduction expansion index, medium-temperature reduction degree, softening temperature, pressure difference steep rise temperature, and dripping temperature requirements.

[0033] In the blast furnace smelting process, the charge is generally composed of a specific proportion of sintered ore and pelletized ore. During the sintering process, a certain proportion of ordinary ore concentrate must be added to the sintered ore to ensure the sintering strength, which limits the upper limit of the use of vanadium-titanium magnetite; while pellets do not have this problem, and can be made from all-vanadium-titanium magnetite concentrate. Therefore, the addition of all-vanadium-titanium magnetite pellets to the furnace can maximize the proportion of vanadium-titanium magnetite and reduce dependence on purchasing high-quality ores.

[0034] In some embodiments, the vanadium-titanium magnetite concentrate accounts for 95-100% of the vanadium-titanium magnetite pellets, wherein the titanium dioxide content in the vanadium-titanium magnetite concentrate is 9-11%, and the vanadium pentoxide (V2O5) content is 0.5-0.75%. In addition, the vanadium-titanium magnetite pellets include additives accounting for 0-5%, and the additives include bentonite and other components.

[0035] In some embodiments, the composition of the vanadium-titanium magnetite concentrate in a typical all-vanadium-titanium magnetite pellet is shown in Table 1, including ferrous oxide (FeO), calcium oxide (CaO), silicon dioxide (SiO2), aluminum oxide (Al2O3), magnesium oxide (MgO), titanium dioxide, vanadium pentoxide, and ferric oxide (Fe2O3). Only ferrous oxide and total iron (TFe) are listed in Table 1, and ferric oxide is not listed. The total iron includes iron in ferric oxide and iron in ferrous oxide, that is, the proportion of the total iron listed is the ratio of the sum of the iron content of ferric oxide and the iron content of ferrous oxide in the vanadium-titanium magnetite concentrate to the vanadium-titanium magnetite concentrate.

[0036] Table 1 Composition of typical vanadium-titanium magnetite concentrate TFe(%) FeO(%) CaO (%) <![CDATA[SiO2(%)]]> <![CDATA[Al2O3(%)]]> MgO (%) <![CDATA[TiO2(%)]]> <![CDATA[V2O5(%)]]> 55~59 32~34 0.2~0.5 2~4 3~3.5 2~33 9~11 0.65~0.75 In some embodiments, the average particle size of the all-vanadium titanium magnetite pellets is 12 to 18 mm, the compressive strength is greater than or equal to 2500N, the roasting conditions are roasting at a temperature above 1250°C for 15 to 25 minutes, the reduction expansion index is less than 15%, the medium-temperature reduction degree is 70 to 75%, the softening temperature is higher than 1150°C, the pressure difference steep rise temperature is higher than 1250°C, and the dripping temperature is maintained at 1450°C ± 10°C.

[0037] In some embodiments, the preparation requirements of the all-vanadium titanium magnetite pellets also include binary basicity R2 and ternary basicity R3 of the all-vanadium titanium magnetite pellets, wherein the binary basicity R2 and ternary basicity R3 of the all-vanadium titanium magnetite pellets are calculated based on the silicon-calcium ratio in the all-vanadium titanium magnetite pellets.

[0038] In some embodiments, the alkaline component includes limestone, and the amount of the alkaline component added is 8-11% of the mass of the vanadium-titanium magnetite concentrate in the all-vanadium-titanium magnetite pellet, that is, the mass ratio of the alkaline component to the vanadium-titanium magnetite concentrate in the all-vanadium-titanium magnetite pellet is 0.08-0.11:1.

[0039] Due to the use of all-vanadium titanium magnetite pellets as furnace charge, the titanium dioxide content in the slag will inevitably increase significantly. According to calculations, under the conditions of all-vanadium titanium magnetite pellet smelting, the titanium dioxide content in the slag can reach more than 40%, which lays the necessary foundation for the subsequent blast furnace slag titanium extraction process. In this way, the comprehensive recovery of iron, vanadium and titanium in vanadium titanium magnetite is truly realized.

[0040] Due to the good rolling performance of all-vanadium titanium magnetite pellets, in order to maintain the central openness and the inverted V-shaped soft melting zone shape, compared with the conventional charge structure (70% sintered ore + 30% pellets), the maximum and minimum distribution angles of all-vanadium titanium magnetite pellets are changed when entering the furnace compared with the conventional charge structure. Due to the fine particle size and large bulk density of all-vanadium titanium magnetite pellets, the permeability of the charge deteriorates when smelting all-vanadium titanium magnetite pellets compared with the conventional charge structure, so a large batch of heavy smelting is required. Studies have shown that the ore-coke interface is one of the main contributors to bed resistance. Smaller-sized pellets will penetrate into the coke gap to form a tighter filling layer. Therefore, it is necessary to reduce the ore-coke interface as much as possible. Under the same smelting conditions, increasing the batch weight of the charge is a means. However, excessive batch weight will lead to an increase in the thickness of the ore layer, a deterioration in the permeability of the soft melting zone, and a decrease in the reducibility of the charge, which is not conducive to the stable operation of the blast furnace. The batch weight of charge corresponds to the sum of the batch weight of ore and the batch weight of coke, but the batch weight of coke is linearly related to the batch weight of ore (generally, the coke ratio needs to be maintained constant), so in some cases the batch weight of charge can also only refer to the batch weight of ore.

[0041] In some embodiments, determining the charge distribution system includes: determining a maximum charge distribution angle and a minimum charge distribution angle and a charge batch weight, wherein the charge batch weight includes an ore batch weight and a coke batch weight.

[0042] In some embodiments, when all-vanadium titanium magnetite pellets are used for smelting, the maximum charge distribution angle is reduced by 1 to 2° compared with smelting using a conventional charge structure, the minimum charge distribution angle is increased by 1 to 2° compared with smelting using a conventional charge structure, and the charge batch weight is increased by 5 to 15% compared with smelting using a conventional charge structure.

[0043] In some embodiments, determining the air supply system includes: solving the air supply system based on local heat and mass balance, calculating the oxygen blowing amount, the furnace tuyere blowing amount, the furnace body blowing amount, the furnace belly gas amount, the furnace cylinder tuyere theoretical combustion temperature, the furnace body gas amount, the gas amount entering the hot blast furnace, the furnace top gas composition, the gas composition entering the hot blast furnace, and pure oxygen blowing in at room temperature without passing through the hot blast furnace.

[0044] In some embodiments, the oxygen injection rate is 220-250 Nm 3 / tHM, furnace tuyere injection volume is 1100~1300Nm 3 / tHM, furnace body injection volume is 600~700Nm 3 / tHM, the amount of gas in the furnace is 1500~1800Nm 3 / tHM, the theoretical combustion temperature of the furnace tuyere is 2000~2200℃, and the gas volume of the furnace is 2000~2500Nm 3 / tHM, the gas volume entering the hot blast furnace is 1700~1900 Nm 3 / tHM.

[0045] In some embodiments, the composition and proportion of the coal gas entering the hot blast furnace are: carbon monoxide, 98%; hydrogen, 1%; nitrogen, 1%.

[0046] In some embodiments, the composition and proportion of the top gas are: carbon monoxide, 85%; carbon dioxide, 14%; nitrogen, 1%.

[0047] In some embodiments, determining the slag making system includes: using self-fluxing all-vanadium titanium magnetite pellets to adjust the binary basicity R2, ternary basicity R3, calcium oxide content, titanium dioxide content, vanadium pentoxide content, magnesium-aluminum ratio, and slag amount of the slag.

[0048] In some embodiments, the binary basicity R2 of the slag is adjusted to 1.3-1.5, the ternary basicity R3 is adjusted to 1.5-1.7, the calcium oxide content is adjusted to 23-28%, the titanium dioxide content is adjusted to 35-40%, the vanadium pentoxide content is adjusted to 0.2-1.0%, the magnesium-aluminum ratio is adjusted to 0.5-0.9, and the slag amount is adjusted to 450-480 kg / tHM (kilograms per ton of iron). The binary basicity R2 and ternary basicity R3 of the slag are calculated based on the silicon-calcium ratio in the slag.

[0049] In some embodiments, determining the thermal regime includes: determining the temperature of the molten iron, and determining the vanadium [V] content, titanium [Ti] content, silicon [Si] content, and sulfur [S] content in the molten iron. [V], [Ti], [Si], and [S] represent vanadium, titanium, silicon, and sulfur in the molten iron, respectively.

[0050] In some embodiments, the molten iron temperature is determined to be 1420-1450° C., the [V] content in the molten iron is determined to be 0.2-0.6%, the [Ti] content is 0.10-0.40%, the [Si] content is 0.10-0.40%, and the [S] content is 0.05-0.20%.

[0051] In some embodiments, determining the operating system includes: determining the material rate according to the blast furnace type selection and batch weight, determining the fuel ratio, the temperature of the heated gas, and determining the wind pressure, wind speed, blast kinetic energy, furnace top pressure, furnace top gas temperature, and setting a waste heat recovery device on the blast furnace top. The fuel ratio includes the coal ratio and the coke ratio, and the total fuel ratio refers to the sum of the coal ratio and the coke ratio.

[0052] In some embodiments, the blast furnace smelting of vanadium-titanium magnetite requires fast in and out, and the material rate is set to be maintained at 8-12 batches / h. The gas temperature after heating is 1150-1200°C, the wind pressure is 370-380kPa, the wind speed is 250-260m / s, the blast kinetic energy is 160-180kJ / s, the furnace top pressure is 190-220kPa, and the furnace top gas temperature is 450-500°C.

[0053] In some embodiments, under the conditions of full oxygen top furnace gas circulation, the solid fuel ratio is reduced by 100 kg / tHM. In order to ensure the permeability of the charge, the coke ratio is maintained at 300-330 kg / tHM, the coal ratio is maintained at 110-150 kg / tHM, and the total fuel ratio is 440-480 kg / tHM. Therefore, the coke load is 5.0-5.7 t / t (ton / ton).

[0054] The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace of the present invention has a furnace capacity of 1750m 3 It is applied in vanadium-titanium magnetite blast furnaces, adopts top gas circulation and full oxygen blast furnace operation, and realizes comprehensive recovery of iron, vanadium and titanium in vanadium-titanium magnetite by adjusting process parameters, material distribution system, air supply system, slag making system, etc. Figure 2 As shown, the furnace gas volume is 1650Nm 3 / tHM, the furnace gas volume is 2476 Nm 3 / tHM, oxygen volume is 240 Nm 3 / tHM, the gas emission into the gas network is 320 Nm 3 / tHM, the gas volume entering the hot blast furnace, i.e. the gas circulation volume, is 1800Nm 3 / tHM, the gas temperature after heating, i.e. the hot air temperature, is 1200℃, and the blowing volume of the furnace tuyere is 1170 Nm 3 / tHM, furnace body injection volume is 630Nm 3 / tHM, furnace tuyere theoretical combustion temperature (TRF) is 2061℃, and furnace top gas temperature is 500℃. The composition and proportion of furnace top gas are: carbon monoxide, 85%; carbon dioxide, 14%; nitrogen, 1%, and the net carbon dioxide removal rate of the whole system is 357 Nm 3 / tHM.

[0055] The components and proportions of the vanadium-titanium magnetite concentrate in the all-vanadium-titanium magnetite pellets are: TFe, 59.01%; FeO, 33.96%; CaO, 0.19%; SiO2, 2.05%; MgO, 1.98%; Al2O3, 2.98%; TiO2, 9.6%; V2O5, 0.74%. The median particle size of the all-vanadium-titanium magnetite pellets is 16mm, the compressive strength is 2517N, the reduction expansion index is less than 12%, the medium-temperature reduction degree is 73%, the softening temperature is 1157℃, the pressure difference steep rise temperature is 1254℃, and the dripping temperature is 1446℃. The material rate is 12 batches / h, the ore batch weight is 47.5t / batch (tons / batch), the coke batch weight is 8.3t / batch, the coke load is 5.7t / t, and the distribution matrix is ​​shown in Table 2 below.

[0056] Table 2 Fabric matrix

[0057] Among them, a represents the angle of the chute, O and C represent ore and coke respectively, sl refers to the depth of the material line, and m is the unit meter. The distribution matrix in Table 2 shows that when the material line depth is controlled to be 2m, the ore is distributed in 0, 2, 3, 3, 2, and 0 circles at chute angles of 39.5°, 38.5°, 37°, 35°, 32.5°, and 26°, respectively. Similarly, coke is distributed in 4, 2, 1, 1, 2, and 4 circles at chute angles of 39.5°, 38.5°, 37°, 35°, 32.5°, and 26°, respectively. The fan-shaped distribution method is realized through the blast furnace distribution chute, the shape of the material surface is controlled, and the central airflow pattern is formed.

[0058] The blast furnace is equipped with 24 tuyere, the length of tuyere is 450mm*20+500mm*4, the diameter of tuyere is 120mm*24, and the air inlet area is 0.2714m 2. The pure oxygen blast temperature is 27°C, the gas pressure after heating is 375kPa, the blast kinetic energy is 177kJ / s, the wind speed in the cyclone zone is 255m / s, the coal ratio is 146kg / tHM, and the coke ratio is 300 kg / tHM. The binary basicity R2 of the slag is 1.31, the ternary basicity R3 is 1.52, the calcium oxide content is 24%, the titanium dioxide content is 35.1%, the vanadium pentoxide content is 0.2-1.0%, the magnesium-aluminum ratio is 0.5-0.9, and the slag volume is 472kg / tHM. The molten iron temperature is 1450°C, the [V] content in the molten iron is 0.46%, the [Ti] content is 0.23%, the [Si] content is 0.3%, and the [S] content is 0.11%.

[0059] Table 3 gives the comparison of the main parameters of the method of smelting all-vanadium titanium magnetite pellets using a full oxygen-carbon cycle blast furnace with the baseline period. After the implementation of the method of the present invention, the solid fuel ratio decreased significantly, with a decrease of 105 kg / tHM, of which the coal ratio decreased by 3 kg / tHM and the coke ratio decreased by 102 kg / tHM. Although the theoretical combustion temperature is 189°C lower than the baseline period, the sensible heat brought in by the furnace gas is reduced, but the furnace body injection promotes the development of indirect reduction in the upper part of the furnace body, resulting in a reduction in the strong endothermic direct reduction in the furnace body + furnace hearth area, which can theoretically meet the iron and slag heating temperature requirements. And from the sensible heat brought into the system by the total reducing gas (i.e., the sensible heat of the furnace gas + the sensible heat of the furnace gas), the sensible heat of the reducing gas in the first stage is increased from 5575MJ / tHM of the traditional blast furnace to 6270MJ / tHM, and the heat supply in the furnace is sufficient. In addition, there is no significant change in the quality of molten iron. On the contrary, due to the decrease in coke ratio (reduced sulfur load) and the increase in furnace oxygen potential, the [S] and [Ti] contents in molten iron also decreased, providing favorable conditions for subsequent vanadium extraction and steelmaking processes. At the same time, the slag volume decreased from 580 kg / tHM in the baseline period to 472 kg / tHM, and the Ti content in the slag increased from 21.3% to 35.1%.

[0060] Table 3 Comparison of main parameters of the full oxygen-carbon cycle blast furnace smelting method of all-vanadium titanium magnetite pellets and the base period

[0061] It can be seen that the method of the present invention can achieve the effect of greatly reducing carbon while significantly reducing the solid fuel ratio, and the Ti in the slag is enriched to 35.1%. Through further quality improvement of the concentrate, it can theoretically reach 40%, laying a foundation for subsequent Ti extraction from slag.

[0062] The method of the present invention adopts full-vanadium titanium magnetite pellets to enter the furnace, which can directly eliminate the sintering process with large carbon emissions and serious pollution, reduce the amount of slag, and reduce the smelting cost and energy consumption; the full oxygen blast reduces the nitrogen in the reducing gas, improves the oxygen potential of the furnace, and reduces the difficulty of separating carbon dioxide in the furnace top gas. The ultra-high reduction potential brought about is also conducive to reducing solid fuel consumption, thereby inhibiting the formation of high-melting point substances such as titanium carbonitride solid solution, and fundamentally solving the problem of smelting high-vanadium titanium ore charge ratio; the carbon circulation of the furnace top gas can achieve ultra-low emissions, and the purified gas is blown through the furnace to replace part of the coal powder or coke consumption; the problem of "cold on top and hot on bottom" of the blast furnace is avoided by blowing the heated gas in stages. Part of the heated coal gas is sprayed through the tuyere of the blast furnace hearth to avoid excessive gas volume in the furnace belly, which may cause liquid flooding and affect smooth operation; the other part is sprayed through the blast furnace body to increase the heat input intensity of the upper part of the furnace body and greatly improve the reduction potential of the furnace body. Using all-vanadium titanium magnetite pellets as the furnace charge, the titanium dioxide content in the slag will inevitably increase significantly, laying the necessary basic conditions for the subsequent blast furnace slag titanium extraction section, and realizing the comprehensive recovery of iron, vanadium and titanium in vanadium titanium magnetite.

[0063] The method of smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace of the present invention is not a splicing and stitching of existing processes, but a process technology route for solving the difficult problem of smelting high-vanadium titanium magnetite ore obtained after theoretical calculation and experimental research, which is interconnected and progressive.

[0064] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0065] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace, characterized in that: include: Pure oxygen is blown into the blast furnace tuyere. After the blast furnace top gas passes through the carbon dioxide separation and capture unit, a part of it enters the gas pipeline network, and the other part is sent to the hot blast furnace for heating. The heated gas is blown into the blast furnace through the hearth tuyere and the body tuyere respectively. The process parameters, charge composition, charge distribution system, air supply system, slag making system, thermal system and operation system are determined. The charge including all-vanadium titanium magnetite pellets is used for blast furnace smelting.

2. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The process parameters are determined by calculating the mass and energy balance of the unit including the furnace belly + furnace hearth, furnace body and hot blast furnace, and the process parameters are determined by adjusting the parameters including the air supply volume of the hot blast furnace, wherein the process parameters include the parameters of the material distribution system, air supply system and heat system.

3. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The method for determining the composition of the charge includes: introducing all-vanadium titanium magnetite pellets into the furnace, and additionally adding alkaline components to cause the all-vanadium titanium magnetite pellets to change from acidic to alkaline, wherein the preparation requirements of the all-vanadium titanium magnetite pellets include the requirements for average particle size, compressive strength, roasting conditions, reduction expansion index, medium-temperature reduction degree, softening temperature, pressure difference steep rise temperature, and dripping temperature.

4. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The determining of the charge distribution system includes: determining the maximum charge distribution angle, the minimum charge distribution angle and the charge batch weight, wherein the charge batch weight includes the ore batch weight and the coke batch weight.

5. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The air supply system is determined by solving the air supply system based on local heat and mass balance, and calculating the oxygen blowing amount, the blowing amount of the furnace tuyere, the blowing amount of the furnace body, the amount of gas in the furnace belly, the theoretical combustion temperature of the furnace tuyere, the amount of gas in the furnace body, the amount of gas entering the hot blast furnace, the gas composition of the furnace top, the gas composition of the gas entering the hot blast furnace, and the blowing of pure oxygen at room temperature without passing through the hot blast furnace.

6. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The slag making system includes: using self-fluxing all-vanadium titanium magnetite pellets to adjust the binary basicity, ternary basicity, calcium oxide content, titanium dioxide content, vanadium pentoxide content, magnesium-aluminum ratio, and slag amount of the slag.

7. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The determination of the thermal system includes: determining the temperature of the molten iron, and determining the vanadium content, titanium content, silicon content, and sulfur content in the molten iron.

8. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 1, characterized in that: The operation system includes: determining the material rate according to the blast furnace type selection and batch weight, determining the fuel ratio, the temperature of the heated gas, and determining the wind pressure, wind speed, blast kinetic energy, furnace top pressure, furnace top gas temperature, and setting a waste heat recovery device on the blast furnace top.

9. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 5, characterized in that: The oxygen volume is 220-250 Nm 3 / tHM, the furnace tuyere injection volume is 1100~1300Nm 3 / tHM, the furnace body injection volume is 600~700Nm 3 / tHM, the furnace gas volume is 1500~1800Nm 3 / tHM, the theoretical combustion temperature of the furnace tuyere is 2000~2200℃, and the gas volume of the furnace body is 2000~2500Nm 3 / tHM, the gas volume entering the hot blast furnace is 1700~1900 Nm 3 / tHM.

10. The method for smelting all-vanadium titanium magnetite pellets in a full oxygen-carbon cycle blast furnace according to claim 6, characterized in that: The binary basicity of the slag is adjusted to 1.3-1.5, the ternary basicity is adjusted to 1.5-1.7, the calcium oxide content is adjusted to 23-28%, the titanium dioxide content is adjusted to 35-40%, the vanadium pentoxide content is adjusted to 0.2-1.0%, the magnesium-aluminum ratio is adjusted to 0.5-0.9, and the slag amount is adjusted to 450-480 kg / tHM.

Citation Information

Cited By

  • Hydrogen and CO2 coupled blast furnace ironmaking method

    CN121951161A