Method for strengthening sulfuric-acid residue oxidized pellets
During the preparation process of oxidized pellets of sulfuric acid slag, the moisture and particle size distribution are controlled to form a multi-layer structure, which solves the problems of poor ball-forming performance of slag slag pellets and large shrinkage after calcination, and improves the oxidized pellets of sulfuric acid slag pellets of sulfuric acid slag pellets of sulfuric acid The compressive strength and metallurgical properties achieve efficient utilization and environmental protection effect of sulfuric acid slag.
Patent Information
- Application Number
- CN202411166849.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-23
AI Technical Summary
In the prior art, the high moisture and fine particle size of sulfuric acid slag lead to serious phenomenon of sticking rollers and wrapping steel balls during sintering, which increases energy consumption and production difficulty. At the same time, the ball-forming performance of sulfuric acid slag is poor, affecting the mechanical strength of the pellets. and compressive strength.
By mixing magnet concentrate powder with binder, adding different proportions of sulfuric acid slags, pelleting, drying, preheating and roasting, controlling the distribution of moisture and particle size, forming a multi-layered and multi-gradient structure to improve sulfuric acid Compressive strength of slag oxidation pellets.
Improve the utilization rate and metallurgical properties of sulfuric acid slag, reduce the cost of pellet ore raw materials, enhance the compressive strength and mechanical properties of oxidized slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag slag s value.
Smart Images

Figure CN118957258A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for strengthening sulphuric acid slag oxidation pellets. Background Art
[0002] Sulfuric acid slag is the roasting slag in the production process of preparing sulfuric acid from pyrite. It is an inevitable product of acid-making chemical plants. At present, there are a large number of sulphuric acid slags all over the country. The rich secondary mineral resources have not been fully and effectively utilized, which not only occupies land resources, but also poses the risk of environmental pollution. Sulfuric acid slag is mainly composed of calcium sulfate, iron oxides, silicates and other components. After a series of sorting and quality improvement, the TFe grade can reach about 60%. The iron oxides are mainly magnetite and hematite, Al2O3 is about 5%, the S content is relatively high, generally around 0.8%, and the content of harmful elements such as K, Pb, and Zn is relatively high. The particle size of sulphuric acid slag is extremely fine, with a particle size of <0.074mm accounting for more than 90%. It has rich microscopic pore structure, strong water absorption, and amorphous structure.
[0003] Sulfuric acid slag is mainly used in cement production, building materials industry, soil conditioner, mine backfill, etc. In the metallurgical industry, sulphuric acid slag is often used as a high-powder raw material in the sintering process. Due to the high S content of sulphuric acid slag, a large amount of S can be removed during the sintering process, but due to its fine particle size and strong water absorption, it has a deteriorating effect on the quality of the sintered ore. The proportion in sintering should not be too high, and the processing consumption capacity is limited. Sulphuric acid slag has fine particle size and large specific surface area. It can be used as an adhesive powder in the process of material balling. Based on the above characteristics, a series of pellets with sulphuric acid slag have been developed. The loose and porous structure of sulphuric acid slag determines its strong water absorption characteristics. The moisture content of the raw ball of the full sulphuric acid slag pellet can reach 23%, which is far higher than the 7~9% of the raw ball of the ordinary pellet ore. Excessive moisture content is not conducive to the drying of the pellets. Therefore, sulphuric acid slag is often added in small amounts to the mixture of iron ore concentrate and binder for pelleting.
[0004] Since the crystal form of sulfate slag grows well after roasting, less primary crystal is formed under high temperature conditions when producing oxidized pellets, the bridge bond consolidation effect is weak, and the compressive strength of the pellets is low. Therefore, it is necessary to strengthen the oxidized pellets of sulfate slag by improving the crystal defects of sulfate slag and improving the spheroidization of sulfate slag. Commonly used methods include adding high-pressure roller grinding and pre-wetting the sulfate slag to improve the spheroidization of the mixture.
[0005] For example, Chinese patent publication number CN101643842 discloses a method for directly using sulfuric acid slag to produce oxidized pellets, which includes pre-treating the sulfuric acid slag with a high-pressure roller mill, adding magnetite concentrate and organic composite bentonite, mixing well, forming pellets, drying and preheating, and oxidizing and roasting to obtain oxidized pellets.
[0006] For example, a Chinese patent with patent publication number CN101597686 discloses a method for preparing a sulfate slag pellet raw material and a method for preparing green pellets, which comprises the following steps: A) taking the sulfate slag and water for the first time to mix to obtain a mixture, wherein the water content of the mixture is 1 WT% to 13 WT%; B) performing a material trapping treatment on the mixture; C) performing a second mixing of the mixture after the material trapping treatment with water and other iron-containing raw materials to obtain a pellet raw material.
[0007] In the above method, a large amount of electric energy is consumed in the process of high-pressure roller grinding, which increases the energy consumption in the production process; under the same rolling conditions, as the moisture content of the iron material increases, the specific surface area and particle size composition after rolling will deteriorate, and when the moisture content of the iron material is too high, it will stick to the roller and the yield will decrease; although the increase in moisture content during lubrication can increase the falling strength of the raw balls, too high moisture content will cause the mixture to wrap around the steel balls and the mixture to stick to the wall seriously, which will bring difficulties to the operation.
[0008] In view of this, improvements should be proposed to the prior art to solve the above-mentioned problems existing in the prior art. Summary of the invention
[0009] The main purpose of the present invention is to provide a method for strengthening sulfate slag oxidation pellets, adding solid waste resource sulfate slag to the pellet raw material to prepare sulfate slag oxidation pellets, thereby improving the utilization rate of sulfate slag, which is beneficial to alleviating the problems of sulfate slag accumulation occupying land and environmental pollution. For low-grade pellet ore, sulfate slag oxidation pellets improve the TFe grade and improve the grade of blast furnace smelting.
[0010] According to one aspect of the present invention, a method for strengthening sulfate slag oxidation pellets is provided, which comprises the following steps: S1, mixing magnetite concentrate powder with a binder to obtain a first mixed ore, mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a second mixed ore, and mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a third mixed ore, wherein the mass proportion of sulfuric acid slag in the second mixed ore is lower than the mass proportion of sulfuric acid slag in the third mixed ore; S2, the first mixed ore is made into a first pellet in a disc pelletizing machine, the second mixed ore is added to the first pellet to make a second pellet, and the third mixed ore is added to the second pellet to make a third pellet; S3, drying, preheating, roasting and cooling the third pellets to obtain sulfate slag oxidation pellets.
[0011] According to one embodiment of the present invention, the TFe grade in the magnetite concentrate powder is 53-56%, and the TFe grade in the sulfate slag is 58-62%.
[0012] According to one embodiment of the present invention, the amount of slag sulfate added to the second mixed ore is 2-6% by mass, and the amount of slag sulfate added to the third mixed ore is 6-10% by mass.
[0013] According to one embodiment of the present invention, the binder includes bentonite, and the amount of the binder added is 1-3% by mass.
[0014] According to one embodiment of the present invention, in step S2, the pelletizing time of the first pelletizing cluster is 5 to 6 minutes, the pelletizing time of the second pelletizing cluster is 8 to 12 minutes, and the pelletizing time of the third pelletizing cluster is 5 to 6 minutes.
[0015] According to one embodiment of the present invention, the moisture content of the first pellet is controlled to be 7-8%, the moisture content of the second pellet is controlled to be 7-9%, and the moisture content of the third pellet is controlled to be 7-10%.
[0016] According to one embodiment of the present invention, the particle size of the first pellet is controlled to be 3-6 mm, the particle size of the second pellet is controlled to be 6-10 mm, and the particle size of the third pellet is controlled to be 10-13 mm.
[0017] According to one embodiment of the present invention, the magnetite concentrate is completely dried, and the particle size <0.074 mm accounts for 90-98%.
[0018] According to one embodiment of the present invention, the sulfuric acid slag is completely dried, and the proportion of particles <0.074 mm is 96-98%.
[0019] According to one embodiment of the present invention, the drying temperature ranges from 100 to 115°C, the preheating temperature ranges from 900°C to 1000°C, and the calcining temperature ranges from 1230°C to 1260°C.
[0020] In a method for strengthening sulfuric acid slag oxidation pellets according to an embodiment of the present invention, sulfuric acid slag, a solid waste resource, is added to the pellet raw material to prepare sulfuric acid slag oxidation pellets, which improves the utilization rate of sulfuric acid slag and is conducive to alleviating the problem of sulfuric acid slag accumulation occupying land and environmental pollution. For low-grade pellets, sulfuric acid slag oxidation pellets improve the TFe grade and improve the blast furnace smelting grade. Sulfate slag, as a solid waste resource, reduces the cost of pellet raw materials. The mother ball is prepared by adding magnetite concentrate and a binder, which reduces the adverse effects caused by the poor balling performance of sulfuric acid slag. The balling process allows the green ball to grow continuously by adding sulfuric acid slag mixtures with different gradient ratios, controls the gradient distribution and density of the green ball moisture, solves the problem of large shrinkage of sulfuric acid slag pellets after roasting, and improves the mechanical strength of the green ball and the compressive strength of the oxidized pellets. The sulfuric acid slag oxidation pellets prepared by this method have qualified compressive strength, good metallurgical properties, and have application and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 A process flow chart of a method for strengthening sulfuric acid slag oxidation pellets according to the present invention is shown; Figure 2 An embodiment of a method for strengthening sulfated slag oxidation pellets according to the present invention is shown. DETAILED DESCRIPTION
[0023] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0024] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.
[0025] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0026] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.
[0027] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.
[0028] Technologies, methods, and apparatus known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and apparatus should be considered part of the specification.
[0029] like Figure 1 As shown, the present invention provides a method for strengthening sulfuric acid slag oxidation pellets, which comprises the following steps: S1, mixing magnetite concentrate powder with a binder to obtain a first mixed ore, mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a second mixed ore, and mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a third mixed ore, wherein the mass proportion of sulfuric acid slag in the second mixed ore is lower than the mass proportion of sulfuric acid slag in the third mixed ore; S2, the first mixed ore is made into a first pellet in a disc pelletizing machine, the second mixed ore is added to the first pellet to make a second pellet, and the third mixed ore is added to the second pellet to make a third pellet; S3, drying, preheating, roasting and cooling the third pellets to obtain sulfate slag oxidation pellets.
[0030] In some specific embodiments, the TFe grade in the magnetite concentrate powder is 53-56%, and the TFe grade in the sulfate slag is 58-62%. The high TFe grade of the magnetite concentrate powder means that the impurity content is relatively low, thereby improving the purity of the product. This is crucial for subsequent smelting, processing and other processes, and can reduce the impact of impurities on product quality.
[0031] In some specific embodiments, the amount of sulphuric acid slag added to the second mixed ore is 2-6% by mass, and the amount of sulphuric acid slag added to the third mixed ore is 6-10%. By adding sulphuric acid slag mixtures of different gradient ratios to promote the continuous and stable growth of green balls, this process requires not only precise control of the proportion of the mixture, but also ensuring that each layer of added sulphuric acid slag can be evenly distributed in the green balls to form a multi-level, multi-gradient structure. The purpose of this is to optimize the pore structure inside the green balls and the binding force between particles by adjusting the physical and chemical properties of each layer of the mixture, such as particle size, density and surface activity.
[0032] In some specific embodiments, the binder includes bentonite, and the amount of the binder added is 1-3% by mass percentage. Sulfate slag is often difficult to form a good sphere alone due to its particular physical and chemical properties, and is prone to problems such as loose spheres, insufficient strength, and easy breakage. Bentonite, as a natural mineral binder, has excellent water absorption, expansion and adhesion, and can significantly improve the ball-forming performance of the mixture. By mixing an appropriate amount of bentonite with magnetite concentrate, the viscosity of the mixture can be significantly improved, so that in the process of preparing the mother ball, the particles can be more closely combined to form a sphere with a dense structure and high strength. This mother ball not only has better physical stability and can resist the impact and wear of external forces, but also can maintain a complete shape during subsequent processing and transportation, reducing breakage and loss. In addition, the addition of bentonite also helps to adjust the moisture distribution and pore structure inside the mother ball, so that the mother ball can better control shrinkage and expansion during roasting or other treatments, and reduce cracks and deformation caused by volume changes. This effect further improves the processing performance of the mother ball and the quality stability of the final product.
[0033] like Figure 2 As shown, in some specific embodiments, in step S2, the pelletizing time of the first pelletizing group is 5-6 minutes, the pelletizing time of the second pelletizing group is 8-12 minutes, and the pelletizing time of the third pelletizing group is 5-6 minutes. For example, the pelletizing time of the first pelletizing group is 5 minutes, the pelletizing time of the second pelletizing group is 10 minutes, and the pelletizing time of the third pelletizing group is 5 minutes.
[0034] In some specific embodiments, the moisture content of the first pellet is controlled to be 7-8%, the moisture content of the second pellet is controlled to be 7-9%, and the moisture content of the third pellet is controlled to be 7-10%. The moisture content of the first pellet, the second pellet and the third pellet increases successively and is distributed in a gradient. The presence of an appropriate amount of water is crucial for the molding, growth and subsequent roasting process of the pellet. By accurately controlling the moisture content of each stage, it can be ensured that the pellet maintains an appropriate degree of wetness during the growth process, and neither the particles are loosely bonded due to being too dry, nor the mechanical strength of the sphere is reduced due to being too wet. At the same time, the gradient distribution of moisture also helps to form a more uniform shrinkage during the roasting process, reducing stress concentration and cracking caused by local moisture differences.
[0035] Appropriate particle size control helps to form a more ideal pore structure, improve the air permeability and roasting performance of the pellets, and is conducive to uniform heating and effective sintering of the pellets in the subsequent processing process. Proper particle size control can also reduce the scrap rate caused by uneven or too large or too small particle size, and improve the qualified rate and economic benefits of the product. In some specific embodiments, the particle size of the first pellet is controlled to be 3-6 mm, the particle size of the second pellet is controlled to be 6-10 mm, and the particle size of the third pellet is controlled to be 10-13 mm.
[0036] In some specific embodiments, the magnetite concentrate is completely dried, and the particle size <0.074 mm accounts for 90-98%, and the sulfate slag is completely dried, and the particle size <0.074 mm accounts for 96-98%. Due to its smaller particle size and higher specific surface area, the particle size <0.074 mm can better adhere together to form a pellet with a dense structure and higher strength. The ball-forming performance of this fine-grained mixed ore is better than that of the coarse-grained one, which helps to reduce the breakage rate of the pellets during production and transportation.
[0037] In some specific embodiments, the drying temperature ranges from 100 to 115°C, the preheating temperature ranges from 900°C to 1000°C, and the calcining temperature ranges from 1230°C to 1260°C.
[0038] In some specific embodiments, the mixed ore is a homogenized ore powder, which can eliminate the composition differences between different batches or different sources of ore powder, so that the whole batch of ore powder has similar chemical composition, particle size and distribution, etc. This uniformity helps to ensure the stability and consistency of product quality in the subsequent production process.
[0039] The present application is described below through specific examples and comparative examples.
[0040] Comparative Example 1 S1. Take completely dried magnetite concentrate powder with a TFe grade of 56% and a particle size of 96% <0.074 mm and mix it with bentonite to obtain a mixed ore powder, in which the mass proportion of magnetite concentrate is 98% and the mass proportion of bentonite is 2%.
[0041] S2. The mixed mineral powder in step S1 is pelletized in a disc pelletizer. The pelletizing time is 20 minutes, the moisture content of the raw balls is 7.9%, and the particle size is 10-13 mm.
[0042] The performance test of the green ball is as follows: the green ball falls 4.5 times / piece, the green ball compressive strength is 9.2N / piece, and the bursting temperature is >600℃.
[0043] S3. After drying the green pellets obtained in step S2, preheat them at 950° C. for 20 min, roast them at 1250° C. for 12 min, and obtain sulfate slag oxidation pellets after cooling.
[0044] The compressive strength test result of the sulfate slag oxidation pellets prepared in Comparative Example 1 is 2541N / piece.
[0045] Comparative Example 2 S1. Take completely dried magnetite concentrate powder with a TFe grade of 56% and a particle size of <0.074mm accounting for 96%, and completely dried sulfate slag with a TFe grade of 59.9% and a particle size of <0.074mm accounting for 98%, and mix them with bentonite to obtain a mixed ore powder, in which the mass proportion of magnetite concentrate is 92%, the mass proportion of sulfate slag is 6%, and the mass proportion of bentonite is 2%.
[0046] S2. The mixed mineral powder in step S1 is pelletized in a disc pelletizer. The pelletizing time is 20 minutes, the moisture content of the raw balls is 9.4%, and the particle size of the raw balls is 10-13 mm.
[0047] The performance test of the green ball is as follows: the green ball falls 4.1 times / piece, the green ball compressive strength is 8.7N / piece, and the bursting temperature is >600℃.
[0048] S3. After drying the green pellets obtained in step S2, preheat them at 950° C. for 20 min, roast them at 1250° C. for 12 min, and obtain sulfate slag oxidation pellets after cooling.
[0049] The compressive strength test result of the sulfate slag oxidation pellets prepared in Comparative Example 2 was 2483N / piece.
[0050] Example 1 S1. Take completely dried magnetite concentrate powder with a TFe grade of 56% and a particle size of 96% <0.074 mm and mix it with bentonite to obtain a first mixed ore powder, wherein the magnetite concentrate accounts for 98% by mass and the bentonite accounts for 2% by mass.
[0051] S2. Take completely dried magnetite concentrate powder with a TFe grade of 56% and a particle size of <0.074 mm accounting for 96%, and completely dried sulfate slag with a TFe grade of 59.9% and a particle size of <0.074 mm accounting for 98%, and mix them with bentonite to obtain a second mixed ore powder, in which the mass proportion of magnetite concentrate is 93%, the mass proportion of sulfate slag is 5%, and the mass proportion of bentonite is 2%.
[0052] S3. Take completely dried magnetite concentrate powder with a TFe grade of 56% and a particle size of <0.074 mm accounting for 96%, and completely dried sulfate slag with a TFe grade of 59.9% and a particle size of <0.074 mm accounting for 98%, and mix them with bentonite to obtain a third mixed ore powder, in which the mass proportion of the magnetite concentrate is 90%, the mass proportion of the sulfate slag is 8%, and the mass proportion of the bentonite is 2%.
[0053] S4. The first mixed ore powder is used to make mother balls in a disc ball making machine. The ball making time is 5 minutes, the moisture content of the mother balls is 7.2%, and the particle size of the mother balls is 3~6mm.
[0054] S5. Add the second mixed ore powder and the third mixed ore powder into the mother ball in turn to make green balls. The ball making time is 10min and 5min respectively. The mass proportion of sulfuric acid slag is 6%. Finally, the moisture content of the green balls is 9.1% and the particle size of the green balls is 10~13mm.
[0055] The performance test of the green ball is as follows: the green ball falls 4.8 times / piece, the green ball compressive strength is 9.8N / piece, and the bursting temperature is >600℃.
[0056] S6. After drying the obtained green pellets, preheat them at 950°C for 20 minutes, roast them at 1250°C for 12 minutes, and obtain sulfate slag oxidation pellets after cooling.
[0057] The compressive strength test result of the sulfate slag oxidation pellets is 2657N / piece.
[0058] This application conducts performance testing on pellets based on standards GB / T14201-2018 "Determination of compressive strength of iron pellets for blast furnace and direct reduction" and GB / T27692-2011 "Acidic iron pellets for blast furnace".
[0059] Table 1 shows the quality of the sulfated slag oxidized pellets in the comparative example and the example.
[0060] Table 1 Quality of sulfuric acid slag oxidation pellets
[0061] The method for strengthening sulfuric acid slag oxidation pellets proposed by the present invention adds sulfuric acid slag, a solid waste resource, to the pellet raw material to prepare sulfuric acid slag oxidation pellets, thereby improving the utilization rate of sulfuric acid slag, and being conducive to alleviating the problems of sulfuric acid slag accumulation occupying land and environmental pollution. For low-grade pellets, sulfuric acid slag oxidation pellets improve the TFe grade and the grade of blast furnace smelting. Sulfic acid slag, as a solid waste resource, reduces the cost of pellet raw materials. The mother ball is prepared by adding magnetite concentrate and a binder, which reduces the adverse effects caused by the poor balling performance of sulfuric acid slag. The balling process allows the green balls to grow continuously by adding sulfuric acid slag mixtures with different gradient ratios, controls the gradient distribution and density of the water content of the green balls, solves the problem of large shrinkage of sulfuric acid slag pellets after roasting, and improves the mechanical strength of the green balls and the compressive strength of the oxidized pellets. The sulfuric acid slag oxidation pellets prepared by the method have qualified compressive strength, good metallurgical properties, and are worth promoting in application.
[0062] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0063] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for strengthening sulfuric acid slag oxidation pelletization, characterized in that: The following steps are involved: S1, mixing magnetite concentrate powder with a binder to obtain a first mixed ore, mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a second mixed ore, and mixing magnetite concentrate powder, sulfuric acid slag and a binder to obtain a third mixed ore, wherein the mass proportion of the sulfuric acid slag in the second mixed ore is lower than the mass proportion of the sulfuric acid slag in the third mixed ore; S2, the first mixed ore is made into a first pellet in a disc pelletizing machine, the second mixed ore is added to the first pellet to make a second pellet, and the third mixed ore is added to the second pellet to make a third pellet; S3, drying, preheating, roasting and cooling the third pellets to obtain sulfate slag oxidation pellets.
2. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The TFe grade in the magnetite concentrate powder is 53-56%, and the TFe grade in the sulfate slag is 58-62%.
3. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: In terms of mass percentage, the amount of the sulfate slag added to the second mixed ore is 2-6%, and the amount of the sulfate slag added to the third mixed ore is 6-10%.
4. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The binder includes bentonite, and the added amount of the binder is 1-3% by mass percentage.
5. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: In step S2, the pelletizing time of the first pelletizing cluster is 5 to 6 minutes, the pelletizing time of the second pelletizing cluster is 8 to 12 minutes, and the pelletizing time of the third pelletizing cluster is 5 to 6 minutes.
6. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The moisture content of the first pellets is controlled to be 7-8%, the moisture content of the second pellets is controlled to be 7-9%, and the moisture content of the third pellets is controlled to be 7-10%.
7. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The particle size of the first pellet is controlled to be 3-6 mm, the particle size of the second pellet is controlled to be 6-10 mm, and the particle size of the third pellet is controlled to be 10-13 mm.
8. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The magnetite concentrate is completely dry, and the particle size <0.074 mm accounts for 90-98%.
9. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The sulfuric acid slag is completely dry, and the particle size of <0.074 mm accounts for 96-98%.
10. The method for strengthening sulfated slag oxidation pellets according to claim 1, characterized in that: The drying temperature ranges from 100 to 115°C, the preheating temperature ranges from 900°C to 1000°C, and the calcining temperature ranges from 1230°C to 1260°C.
Citation Information
Patent Citations
Method for strengthening oxidized pellet prepared by directly using sulfate slag
CN101643842A
Pyrite cinder composite pellet and preparation method thereof
CN101985688A
Method for improving strength of pellets
CN103451416A
Method for harmlessly treating electroplating sludge in metallurgical sintering blast furnace
CN104152682A
Method for producing pellets by mixing vanadium titano-magnetite and sulfuric-acid residues
CN116463495A