Se-doped Zintl phase thermoelectric material BaCu2Te2 preparation method
Through simplified preparation methods, including Ba ingot smelting, solid phase reaction and hot press sintering, the complex problem of the preparation process of BaCu2Te2 thermoelectric material is solved, and the preparation of high-performance Zintl phase thermoelectric material BaCu2Te2 doped Se is realized, which improves the conductance of the material Rate and power factor performance.
Patent Information
- Application Number
- CN202411029298.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The preparation process of existing BaCu2Te2 thermoelectric materials is complex, which limits its performance optimization and large-scale application.
A simplified preparation method is adopted, including smelting of Ba ingots, proportional preparation with Cu strips and Te blocks, solid phase reaction and annealing in an argon environment, grinding and hot press sintering, ensuring the purity and performance optimization of the sample.
The preparation process is simplified, the conductivity and power factor performance of the material are improved, and the characteristics of the Zintl phase material are in line with the performance of the Zintl phase material, achieving efficient thermoelectric performance.
Smart Images

Figure CN118957336A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermoelectric materials, and more specifically, to a method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se. Background Art
[0002] High-performance thermoelectric materials need to have both high electrical transport performance and low thermal transport performance. However, the strongly coupled electroacoustic properties make it very difficult to regulate the transport of electrons or phonons alone, which is also the main reason that limits the improvement of thermoelectric figure of merit. In 1995, Slack proposed a design criterion for thermoelectric materials based on basic physical properties, believing that good thermoelectric materials should have glass-like thermal conductivity and single crystal-like electrical properties, namely "phonon glass-electron crystal" (PGEC). Under the guidance of this theory, people have discovered materials with "phonon glass-electron crystal" characteristics such as filled skutterudite compounds and intermetallic complexes, and have achieved excellent thermoelectric performance. Among them, Zintl phase alloys have low intrinsic lattice thermal conductivity due to their complex crystal structure. At the same time, the covalent grid in the crystal provides a good channel for electrical transport, which is a very promising class of thermoelectric materials.
[0003] Compared with other Zintl materials, 1-2-2Zintl phase BaCu2Te2 material combines its internal complex bonding structure and crystal structure, so that it has high electrical conductivity, naturally low lattice thermal conductivity and high carrier mobility, and has excellent thermoelectric performance. At the same time, it has the characteristics of copper-based materials, and its thermoelectric performance can be further regulated on this basis to further optimize its thermoelectric performance. However, the current preparation process and process of BaCu2Te2 are complicated. In view of this, the inventors propose a preparation method of Zintl phase thermoelectric material BaCu2Te2 doped with Se. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se, thereby simplifying the preparation process and flow of BaCu2Te2.
[0005] 2. The above technical objectives of the present invention are achieved through the following technical solutions: A method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se, comprising the following steps:
[0006] S1. First, the Ba ingot is smelted to remove oxygen elements and impurities in the Ba ingot for purification;
[0007] S2, weigh the smelted Ba ingot, Cu bar, Te block and Se powder in proportion in a glove box, cut the raw materials into pieces, put them into a crucible with a cover, and then put the crucible into a glass tube;
[0008] S3. To avoid oxidation of the sample, a vacuum valve was applied to the glass tube to isolate the air and keep the glass tube filled with argon. The glass tube in the glove box was taken out and sealed in an ice bath vacuum.
[0009] S4, placing the sealed glass tube into a muffle furnace for solid phase reaction;
[0010] S5. Take out the glass tube and put it into the glove box, take out the sample, and grind it with a mortar for half an hour to make the sample fully uniform and into a fine powder;
[0011] S6. Continue to put the sample into the crucible, and then into the glass tube;
[0012] S7, putting a vacuum valve on the glass tube in the glove box and sealing the tube by ice bath vacuum;
[0013] S8, placing the sealed glass tube into a muffle furnace for annealing;
[0014] S9. Take out the glass tube and put it into the glove box, take out the sample, and grind it with a mortar for half an hour to make the sample more fully and evenly into a fine black powder;
[0015] S10, perform powder XRD test and compare with standard PDF card to determine whether the sample is BaCu2Te2;
[0016] S11. Sintering the powder into a solid by hot pressing.
[0017] The present invention is further configured as follows: in step S2, the ratio of the Ba ingot, the Cu strip and the Te block is 1:2:2, Se is doped at the Te position, and the Se doping ratio is 0.06.
[0018] The present invention is further configured as follows: in step S4, the temperature setting of the solid phase reaction is specifically as follows: rising from room temperature to 450°C for 10 hours and keeping the temperature for 10 hours, rising from 450°C to 600°C for 10 hours and keeping the temperature for 10 hours, rising from 600°C to 900°C for 10 hours and keeping the temperature for 3 days, and finally cooling to room temperature with the furnace;
[0019] The present invention is further configured as follows: in step S8, the specific temperature and time of the annealing are: from room temperature to 750°C at a rate of 1.3°C / min and kept for 3 days, and finally cooled to room temperature with the furnace.
[0020] The present invention is further configured as follows: in step S11, the parameters of the hot pressing are: pressure 75 MPa, temperature 600° C., and sintering time 35 min.
[0021] In summary, the present invention has the following beneficial effects: The present invention explores a method for synthesizing BaCu2Te2 and simplifies the preparation process and flow. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a flow chart of the preparation method of Zintl phase thermoelectric material BaCu2Te2;
[0023] Figure 2 This is the XRD test result diagram of the BaCu2Te2 Se-doped sample of the present invention;
[0024] Figure 3 This is the SEM test result of BaCu2Te2 doped with Se0.06 sample Figure 1 ;
[0025] Figure 4 This is the SEM test result of BaCu2Te2 doped with Se0.06 sample Figure 2 ;
[0026] Figure 5 This is the conductivity data result diagram of BaCu2Te2 doped with Se0.06 sample;
[0027] Figure 6 This is the Seebeck data result diagram of BaCu2Te2 doped with Se0.06 sample;
[0028] Figure 7 This is the power factor data result diagram of BaCu2Te2 doped with Se0.06 sample. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example:
[0031] A method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se, such as Figure 1 As shown, the following steps are included:
[0032] S1. First, the Ba ingot is smelted to remove oxygen and impurities in the Ba ingot to achieve the purpose of purification for the next experiment. Since Ba metal is very easy to oxidize, it is best not to contact with air before and after smelting to avoid oxidation;
[0033] S2. Since Ba metal is very easy to oxidize, weighing and sampling are carried out in a glove box: the smelted Ba ingot, Cu bar, and Te block are weighed in proportion, the raw materials are cut into pieces, and Se powder is added to facilitate fusion, and then put into a crucible with a lid, and then the crucible is placed in a glass tube. The ratio of Ba ingot, Cu bar, and Te block is 1:2:2, Se is doped at the Te position, and the Se doping ratio is 0.06;
[0034] S3. To avoid oxidation of the sample, a vacuum valve can be applied to the glass tube to isolate the air and keep the glass tube filled with argon. Then the glass tube is taken out of the glove box and sealed in an ice bath vacuum (if there are raw materials with low melting points in the sample, ice bath protection is used when sealing the tube);
[0035] S4, put the sealed glass tube into a muffle furnace for solid phase reaction at a temperature of 900°C. (Specific temperature and time: from room temperature to 450°C for 10h and keep it for 10h, from 450°C to 600°C for 10h and keep it for 10h, from 600°C to 900°C for 10h and keep it for 3 days, and finally cool it to room temperature with the furnace);
[0036] S5. Considering that some raw materials may not react completely in one reaction, to avoid oxidation, put the taken out glass tube into the glove box, take out the sample in the crucible, and grind it with a mortar for half an hour to make the sample fully uniform and into a fine powder;
[0037] S6. Put the ground sample back into the crucible and then into the glass tube;
[0038] S7, put a vacuum valve on the glass tube in the glove box, take it out and seal it in an ice bath vacuum;
[0039] S8. Place the sealed glass tube into a muffle furnace for annealing at a temperature of 750°C; (Specific temperature and time: from room temperature to 750°C at a rate of 1.3°C / min and keep at this temperature for 3 days, and finally cool to room temperature with the furnace)
[0040] S9. To avoid oxidation, put the glass tube into the glove box, take out the sample from the crucible, and grind it with a mortar for half an hour to make the sample more uniform and into a fine black powder.
[0041] S10, take out some samples, perform powder XRD test, compare with standard PDF card, determine whether the sample is BaCu2Te2; the test results are as follows Figure 2 As shown;
[0042] S11. To continue the thermoelectric material performance test, the powder is sintered into a dense solid by hot pressing, the hot pressing pressure is 75Mpa, the temperature is 600℃, and the sintering time is 35min (the pressure should be removed immediately after the heat preservation). That is, the sample preparation is completed.
[0043] The samples obtained above were subjected to SEM test, and the test results are as follows: Figure 3 and Figure 4 As shown, Te, Cu, Ba, and Se elements are evenly distributed.
[0044] The electrical properties of the Se0.06-doped sample were tested for conductivity, Seebeck, and power factor. The test results are as follows: Figure 5 , Figure 6 and Figure 7 As shown, the sample material has good electrical properties, high conductivity, high Seebeck coefficient, and very good power factor value, which is consistent with the electronic crystal characteristics of Zintl phase material.
[0045] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se, characterized in that: The steps include: S1. First, the Ba ingot is smelted to remove oxygen elements and impurities in the Ba ingot for purification; S2, weigh the smelted Ba ingot, Cu bar, Te block and Se powder in proportion in a glove box, cut the raw materials into pieces, put them into a crucible with a cover, and then put the crucible into a glass tube; S3. To avoid oxidation of the sample, a vacuum valve was applied to the glass tube to isolate the air and keep the glass tube filled with argon. The glass tube in the glove box was taken out and sealed in an ice bath vacuum. S4, placing the sealed glass tube into a muffle furnace for solid phase reaction; S5. Take out the glass tube and put it into the glove box, take out the sample, and grind it with a mortar for half an hour to make the sample fully uniform and into a fine powder; S6. Continue to put the sample into the crucible, and then into the glass tube; S7, putting a vacuum valve on the glass tube in the glove box and sealing the tube by ice bath vacuum; S8, placing the sealed glass tube into a muffle furnace for annealing; S9. Take out the glass tube and put it into the glove box, take out the sample, and grind it with a mortar for half an hour to make the sample more fully and evenly into a fine black powder; S10, perform powder XRD test and compare with standard PDF card to determine whether the sample is BaCu2Te2; S11. Sintering the powder into a solid by hot pressing.
2. The method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se according to claim 1, characterized in that: In step S2, the ratio of the Ba ingot, the Cu strip and the Te block is 1:2:2, Se is doped at the Te position, and the Se doping ratio is 0.
06.
3. The method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se according to claim 1, characterized in that: In step S4, the temperature setting of the solid phase reaction is specifically as follows: from room temperature to 450°C for 10 hours and keep warm for 10 hours, from 450°C to 600°C for 10 hours and keep warm for 10 hours, from 600°C to 900°C for 10 hours and keep warm for 3 days, and finally cooling to room temperature with the furnace.
4. The method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se according to claim 1, characterized in that: In step S8, the specific temperature and time of the annealing are: from room temperature to 750°C at 1.3°C / min and kept for 3 days, and finally cooled to room temperature in the furnace.
5. The method for preparing a Zintl phase thermoelectric material BaCu2Te2 doped with Se according to claim 1, characterized in that: In step S11, the hot pressing parameters are: pressure 75 MPa, temperature 600° C., and sintering time 35 min.