Tungsten-cobalt hard alloy sintering process
By employing multi-layer coating and spark plasma sintering processes, the problems of internal porosity and abnormal grain growth in tungsten-cobalt cemented carbide have been solved, resulting in a high-density and homogeneous alloy that improves hardness and wear resistance, making it suitable for manufacturing high-load tools.
Patent Information
- Application Number
- CN202411067415.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sintering techniques are insufficient to completely eliminate internal porosity and defects in tungsten-cobalt cemented carbide, and abnormal grain growth leads to performance degradation.
By employing multilayer coating technology and spark plasma sintering process, and by controlling the heating rate, sintering temperature, holding time, and internal pressure, combined with the gradient distribution of inhibitors, a high-density and uniform tungsten-cobalt cemented carbide was prepared.
It improves the density and uniformity of tungsten-cobalt cemented carbide, inhibits abnormal growth of pores and grains, and enhances the hardness and wear resistance of the alloy, making it suitable for tool manufacturing under high load and high wear environments.
Smart Images

Figure CN118957341A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy sintering, and in particular relates to a sintering process of tungsten-cobalt cemented carbide. Background Art
[0002] Cemented carbide, especially tungsten-cobalt cemented carbide, has been widely used in cutting tools, wear-resistant tools and mining tools due to its excellent hardness, wear resistance, strength and fracture toughness. Tungsten-cobalt cemented carbide is mainly composed of tungsten carbide (WC) and metallic cobalt (Co). The cobalt content varies between 3% and 30%. The WC grain size in the alloy is also different according to the specific application requirements.
[0003] In the production process of cemented carbide, sintering process is the key link that determines product quality. Traditional sintering methods include vacuum sintering, vacuum post-hot isostatic pressing sintering, etc. These methods meet production needs to a certain extent, but there is still room for improvement. In recent years, with the development of materials science and manufacturing technology, some new sintering methods such as microwave sintering and spark plasma sintering (SPS) have gradually entered the research field of vision. These technologies, with their unique heating methods and rapid heating characteristics, show the potential to improve product quality and production efficiency.
[0004] However, the existing sintering technology still has some shortcomings, such as the difficulty in completely eliminating the pores and defects inside the sintered body, the abnormal growth of grains during the sintering process leading to performance degradation, etc. Therefore, a tungsten-cobalt cemented carbide sintering process is proposed to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a sintering process of tungsten-cobalt cemented carbide to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a sintering process of tungsten-cobalt cemented carbide, comprising the following steps:
[0007] S1: Tungsten carbide powder and metal cobalt powder are mixed in a preset ratio, and inhibitors are added through multi-layer coating, and then forming agents are added, followed by wet grinding and drying processes, and finally pressed into compacts;
[0008] S2: Dewaxing and pre-burning the compact in a vacuum environment to remove the forming agent and perform preliminary sintering;
[0009] S3: placing the pre-sintered compact in a spark plasma sintering furnace, and performing spark plasma sintering under vacuum or inert gas protection, and rapidly densifying the cemented carbide by controlling the heating rate, sintering temperature, holding time and internal pressure;
[0010] S4: After sintering, the alloy is cooled in multiple stages. After complete cooling, the cemented carbide is pre-treated to obtain the final product.
[0011] Preferably, the heating rate is 10°C to 200°C / min, the sintering temperature is 1100°C to 1300°C, the holding time is 5min to 30min, and the internal pressure is 0MPa to 60MPa.
[0012] Preferably, the multi-stage cooling includes furnace cooling and air cooling.
[0013] Preferably, the purity of the tungsten carbide powder and the metal cobalt powder is ≥ 99%.
[0014] Preferably, the pretreatment in S4 includes cleaning and polishing.
[0015] Preferably, the inhibitor comprises vanadium carbide, chromium carbide and tantalum carbide.
[0016] Preferably, the molding agent includes paraffin, zinc stearate, and polyvinyl alcohol.
[0017] Preferably, the ratio of the tungsten carbide powder to the metal cobalt powder is 92% to 97%; 3% to 8%.
[0018] Preferably, the multi-layer coating and adding inhibitor specifically comprises the steps of:
[0019] S11: mixing the pretreated inhibitor powder with a portion of tungsten carbide powder and metal cobalt powder, and forming a first coating layer on the powder surface by wet ball milling and spray drying;
[0020] S12: Repeat S11 to form one or more coating layers on the surface of the coated powder;
[0021] S13: After all the intermediate layers are coated, the remaining tungsten carbide powder and metal cobalt powder are mixed with the last layer of inhibitor powder for final coating.
[0022] Preferably, the pretreatment includes chemical plating and physical vapor deposition.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The tungsten-cobalt cemented carbide prepared by the present invention through multi-layer coating and spark plasma sintering has higher density and uniformity. At the same time, the gradient distribution of the inhibitor effectively improves the hardness and wear resistance of the alloy, avoids the phenomenon that the pores and defects inside the sintered body are difficult to completely eliminate and the abnormal grain growth during the sintering process. It is suitable for tool manufacturing in high-load and high-wear environments. By optimizing the type and proportion of inhibitors and increasing the sintering temperature and holding time, the prepared tungsten-cobalt cemented carbide significantly improves the wear resistance while maintaining high hardness. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] See also Figure 1 As shown, the present invention provides the following technical solutions:
[0028] Embodiment 1:
[0029] Raw material preparation: 99.5% pure tungsten carbide powder and 99.9% pure cobalt powder are mixed at a mass ratio of 95:5. At the same time, vanadium carbide, chromium carbide and tantalum carbide are prepared as inhibitors, mixed in a certain proportion and pre-treated (such as chemical plating) to enhance their dispersibility.
[0030] Multi-layer coating: Multi-layer coating is performed. First, the pre-treated inhibitor powder is mixed with 20% tungsten carbide powder and metal cobalt powder, and the first coating layer is formed by wet ball milling and spray drying. Subsequently, this process is repeated, and two more layers of inhibitor coating are added, with slightly different inhibitor types and proportions used in each layer to achieve a gradient effect. Finally, the remaining tungsten carbide powder and metal cobalt powder are mixed with the last layer of inhibitor to complete the final coating.
[0031] Wet grinding, drying and pressing: Add an appropriate amount of paraffin wax as a molding agent to the coated powder, wet grind it to a uniform particle size, and then dry and press it into a compact.
[0032] Dewaxing and pre-firing: Dewaxing and pre-firing are carried out in a vacuum environment to remove the forming agent and perform preliminary sintering.
[0033] Spark plasma sintering: The pre-sintered compact is placed in a spark plasma sintering furnace and heated to 1200°C at a heating rate of 150°C / min under vacuum, kept at that temperature for 15 minutes, and the internal pressure is maintained at 30MPa to achieve rapid densification.
[0034] Multi-stage cooling and post-processing: After sintering, the alloy is first cooled to 600°C in the furnace and then air-cooled to room temperature. Finally, the alloy is cleaned and polished to obtain the final product.
[0035] Example 2
[0036] Raw material preparation: 99.9% pure tungsten carbide powder and metal cobalt powder are mixed at a mass ratio of 97:3. A high proportion of tantalum carbide is selected as an inhibitor because of its excellent wear resistance.
[0037] Multilayer cladding: Similar to Example 1, but increasing the proportion of tantalum carbide in the final cladding layer to further enhance the wear resistance of the alloy.
[0038] Sintering and cooling: During the spark plasma sintering process, the sintering temperature is increased to 1300°C and the holding time is extended to 20 minutes to further promote the densification and grain refinement of the alloy. The cooling process still adopts a combination of furnace cooling and air cooling.
[0039] Example 3
[0040] Raw material preparation: Use tungsten carbide powder with a purity of 99.5% and a lower proportion of metal cobalt powder (mass ratio of 92:8) to reduce the alloy cost while maintaining certain mechanical properties.
[0041] Multilayer cladding: Considering the low cobalt content, the total addition of inhibitors is increased, especially vanadium carbide and chromium carbide, to enhance the strength and toughness of the alloy.
[0042] Sintering and post-treatment: During the spark plasma sintering process, the heating rate and internal pressure are strictly controlled to ensure uniform densification of the alloy. After sintering, strict cleaning and polishing are carried out to improve the surface quality of the alloy.
[0043] Example 4
[0044] Preparation of nano-inhibitors: First, prepare nano-scale vanadium carbide, chromium carbide and tantalum carbide powders by chemical synthesis or physical pulverization to ensure that the particle size is below 50nm.
[0045] Multilayer coating: The nano-inhibitor powder is evenly dispersed in the solvent, and then multi-layer coated with tungsten carbide powder and metal cobalt powder (ratio 94:6) by spray drying. Due to the high specific surface area and activity of the nano-inhibitor, it can more effectively promote the densification and performance improvement of the alloy.
[0046] Sintering process: Spark plasma sintering technology is used to sinter under vacuum or inert gas protection. The heating rate is set to 100℃ / min, the sintering temperature is 1250℃, the holding time is 10 minutes, and the internal pressure is controlled at 40MPa.
[0047] Post-processing: After sintering, multi-stage cooling is carried out, followed by ultrasonic cleaning and fine polishing to remove surface impurities and improve appearance quality.
[0048] Example 5
[0049] Raw material layering: Divide tungsten carbide powder and metal cobalt powder into several layers according to different ratios, such as 97:3, 95:5, and 93:7 from the center to the edge, to create a gradient density structure.
[0050] Multi-layer coating and pressing: Each layer of raw material is subjected to multi-layer coating treatment, and an appropriate amount of inhibitor (such as vanadium carbide and chromium carbide) is added. Subsequently, these layered coated powders are placed in a mold in turn and pressed to form a compact with a gradient density.
[0051] Sintering process: The compact is sintered in a spark plasma sintering furnace. The sintering parameters of each layer (such as heating rate, sintering temperature and holding time) are adjusted to ensure good metallurgical bonding between the layers while retaining their gradient density characteristics.
[0052] Post-processing: After sintering, multiple cooling stages and conventional post-processing steps (such as cleaning and polishing) are performed.
[0053] Example 6
[0054] Environmentally friendly molding agent selection: biodegradable polylactic acid (PLA) or starch-based molding agents are used to replace traditional non-degradable materials such as paraffin.
[0055] Mixing and pressing: After the pretreated tungsten carbide powder, metal cobalt powder and inhibitor powder are evenly mixed, an appropriate amount of environmentally friendly forming agent is added for wet grinding and pressing to form a compact.
[0056] Sintering and removal of molding agent: Sintering is carried out under vacuum or inert gas protection. Since the environmentally friendly molding agent has a low decomposition temperature, it can be effectively removed at the beginning of sintering without negatively affecting the properties of the alloy.
[0057] Subsequent treatment: After sintering, multiple cooling and conventional post-processing steps are carried out. In particular, due to the degradability of the forming agent, there is no need to worry about environmental pollution.
[0058] Example 7
[0059] Microstructure design: By optimizing the size distribution of tungsten carbide particles, an appropriate amount of ultrafine tungsten carbide particles (particle size less than 0.5 microns) are introduced and mixed with conventional tungsten carbide particles to improve the toughness of the alloy.
[0060] Multi-layer coating: Add an appropriate amount of toughness enhancer (such as zirconium carbide or nano-graphite) to the mixed powder, and use multi-layer coating technology to evenly distribute these enhancers on the surface of tungsten carbide and cobalt powder.
[0061] Sintering process: A two-step sintering method is used, firstly low-temperature pre-sintering is carried out to promote the initial bonding between powders, followed by high-temperature sintering to achieve densification. During the sintering process, the heating rate and holding time are precisely controlled to reduce grain growth and retain the toughness phase in the microstructure.
[0062] Post-treatment: After sintering, multi-stage cooling and surface strengthening treatment (such as carburizing or nitriding) are carried out to further improve the hardness and wear resistance of the alloy while maintaining its toughness.
[0063] Example 8
[0064] Powder mixing and pressing: After tungsten carbide powder, metal cobalt powder and inhibitor powder are mixed evenly in a preset ratio, they are pressed to form a compact.
[0065] Hot isostatic pressing pretreatment: The compact is placed in a hot isostatic pressing device and pretreated at a lower temperature and pressure to promote initial bonding between powders and reduce shrinkage during sintering.
[0066] Spark plasma sintering: After hot isostatic pressing pretreatment, the compact is transferred to the spark plasma sintering furnace for final sintering. Since the pretreatment improves the bonding state between the powders, the temperature and pressure conditions during the sintering process can be further optimized to obtain higher density and performance.
[0067] Post-processing: After sintering, conventional multi-stage cooling and post-processing steps are carried out.
[0068] Example 9
[0069] Layered mixing: Tungsten carbide powder and metal cobalt powder are layered and mixed according to different particle size distributions to form a raw material layer with a gradient grain size distribution.
[0070] Multi-layer coating: Add appropriate amount of inhibitors and grain refiners (such as carbon black or rare earth elements) to each layer of raw materials, and distribute these additives evenly on the powder surface through multi-layer coating technology.
[0071] Sintering process: Gradient temperature rise sintering method is adopted, that is, different temperature gradients are set in different sintering stages to promote differentiated sintering and grain growth of each layer of raw materials. By precisely controlling the sintering parameters, a structure with gradient grain size distribution is achieved.
[0072] Post-processing: After sintering, multi-stage cooling and necessary surface treatment are carried out.
[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A sintering process of tungsten-cobalt cemented carbide, characterized in that: The steps include: S1: Tungsten carbide powder and metal cobalt powder are mixed in a preset ratio, and inhibitors are added through multi-layer coating, and then forming agents are added, followed by wet grinding and drying processes, and finally pressed into compacts; S2: Dewaxing and pre-burning the compact in a vacuum environment to remove the forming agent and perform preliminary sintering; S3: placing the pre-sintered compact in a spark plasma sintering furnace, and performing spark plasma sintering under vacuum or inert gas protection, and rapidly densifying the cemented carbide by controlling the heating rate, sintering temperature, holding time and internal pressure; S4: After sintering, the alloy is cooled in multiple stages. After complete cooling, the cemented carbide is pre-treated to obtain the final product.
2. A sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: In S3, the heating rate is 10°C to 200°C / min, the sintering temperature is 1100°C to 1300°C, the holding time is 5min to 30min, and the internal pressure is 0MPa to 60MPa.
3. A sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: In S4, the multi-stage cooling includes furnace cooling and air cooling.
4. A sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: In S1, the purity of the tungsten carbide powder and the metal cobalt powder is ≥ 99%.
5. The sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: The pretreatment in S4 includes cleaning and polishing.
6. The sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: The inhibitors include vanadium carbide, chromium carbide and tantalum carbide.
7. The sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: The molding agent includes paraffin, zinc stearate and polyvinyl alcohol.
8. The sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: The ratio of the tungsten carbide powder to the metal cobalt powder is 92% to 97%; 3% to 8%.
9. The sintering process of tungsten-cobalt cemented carbide according to claim 1, characterized in that: In S1, the multi-layer coating adding inhibitor specifically comprises the steps of: S11: mixing the pretreated inhibitor powder with a portion of tungsten carbide powder and metal cobalt powder, and forming a first coating layer on the powder surface by wet ball milling and spray drying; S12: Repeat S11 to form one or more coating layers on the surface of the coated powder; S13: After all the intermediate layers are coated, the remaining tungsten carbide powder and metal cobalt powder are mixed with the last layer of inhibitor powder for final coating.
10. A sintering process of tungsten-cobalt cemented carbide according to claim 9, characterized in that: In S11, the pretreatment includes chemical plating and physical vapor deposition.
Citation Information
Cited By
Preparation method and device of gradient structure tungsten carbide-cobalt composite grinding ball for ball mill
CN120619359A
Preparation method of hard alloy
CN121802263A