Cast aluminum alloy composite refining agent and preparation method thereof

By using composite refining agents with NaCl, NaF, TiCl3, SrSO4, KPO3, Na2B4O7 and other components, the existing cast aluminum alloy refining agent has solved the problems of low gas removal efficiency and environmental pollution, and achieved efficient and environmentally friendly aluminum alloy refining The effect significantly improves the cleanliness and mechanical properties of aluminum alloy.

CN118957342APending Publication Date: 2024-11-15GUANGDONG ENG POLYTECHNIC COLLEGE +1

Patent Information

Application Number
CN202410995454.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing cast aluminum alloy refining agent has low gas removal efficiency and a single function. It has large irritating smoke emissions during use, resulting in poor separation of environmental pollution and aluminum slag, making it difficult to meet the production of high-clean and high-performance cast aluminum alloys. need.

Method used

Compound refining agents with NaCl, NaF, TiCl3, SrSO4, KPO3, Na2B4O7 and other components were prepared by solution evaporation to form eutectics with low melting points, enhance the degassing function, and refine α during the solidification process of aluminum alloy. -Al grains, Si phase and Fe-rich phase to reduce smoke emissions.

Benefits of technology

It significantly improves the cleanliness and mechanical properties of cast aluminum alloys, reduces aluminum slag emissions, reduces environmental pollution, and achieves more efficient degassing and slag removal effects and environmentally friendly use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957342A_ABST
    Figure CN118957342A_ABST
Patent Text Reader

Abstract

The invention discloses a cast aluminum alloy composite refining agent and a preparation method thereof, and belongs to the technical field of cast aluminum alloy refining and modification. According to the technical scheme, the refining agent is characterized by being prepared from, by mass, 34%-36% of NaCl, 18%-22% of NaF, 15%-17% of TiCl3, 8%-12% of SrSO4, 9%-13% of KPO3 and 6%-8% of Na2B4O7. The preparation method comprises the steps of burdening, evaporative crystallization, crushing and drying dehydration. The refining agent overcomes the problems of low degassing and deslagging efficiency, large smoke discharge amount, poor slag-aluminum separation effect, single function and the like of a traditional refining agent, has excellent degassing and deslagging effects, can remarkably reduce the gas and slag content of cast aluminum alloy liquid, also has a refining and modification effect on cast aluminum alloy, and is suitable for industrial production. The harm of pores, inclusions and thick second phases to the mechanical property of the cast aluminum alloy can be eliminated, and the casting fluidity and mechanical property of the aluminum alloy are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refining and modification of cast aluminum alloys, and in particular relates to a composite refining agent for cast aluminum alloys and a preparation method thereof. Background Art

[0002] Cast aluminum alloy is an aluminum alloy with aluminum and silicon as the main elements. It has good casting performance, corrosion resistance and mechanical properties. It is widely used in casting various aluminum alloy parts, such as engine cylinder block, cylinder head, piston, wheel, etc. The performance of cast aluminum alloy is closely related to its cleanliness. Porosity and inclusions will split the matrix of cast aluminum alloy, destroy the organizational continuity of cast aluminum alloy, cause local stress concentration, become the crack source and crack propagation direction of cast aluminum alloy fracture, thereby reducing the strength and plasticity of cast aluminum alloy. The performance of cast aluminum alloy is also closely related to the morphology and size of its α-Al grains, Si phase and Fe-rich phase. Coarse α-Al grains, Si phase and Fe-rich phase will reduce the fluidity, strength and plasticity of cast aluminum alloy, while fine and uniform α-Al grains, Si phase and Fe-rich phase can improve the fluidity, strength and plasticity of cast aluminum alloy. Therefore, during the smelting process, the casting aluminum alloy liquid must be refined, degassed, deslaged and refined to reduce the gas and slag content of the casting aluminum alloy and refine the α-Al grains, Si phase and Fe-rich phase of the casting aluminum alloy.

[0003] The invention patent with publication number CN102286667A discloses a sodium-free refining agent for aluminum and aluminum alloys and a production method thereof. The refining agent is composed of the following components in mass percentage: 15-25% potassium fluoroaluminate, 5-15% calcium fluoride, 10-25% potassium carbonate, 10-25% potassium sulfate, 5-15% barium sulfate, 15-30% potassium chloride, and 3-5% anhydrous aluminum chloride. The production method includes raw material screening, batching, mixing, testing and packaging.

[0004] The invention patent with publication number CN86105179A discloses a modification and refining agent for aluminum silicon alloy, which is composed of the following components in mass percentage: NaCl 20-40%, NaF 40-60%, Na3AlF65-15%, Na2SiF6 5-15%, or NaCl 20-30%, NaF 45-65%, Na2SiF6 15-25%. The modification and refining agent is composed of multiple sodium salts and has the functions of refining, purifying, refining and modification.

[0005] The invention patent with publication number CN85100320A discloses a long-lasting flux for aluminum-silicon alloy, which is made by mixing and pressing the following components in mass percentage: SrCO3 10-15%, Mg powder 6-10%, Sr(NO2)28-12%, NaNO3 8-12%, K2CO3 18-25%, carbon powder 2-5%, refractory brick powder 25-30%, and catalyst 8-12%. The flux realizes the composite modification of Na salt and Sr salt and the integration of modification and refining.

[0006] According to the results of literature retrieval and production practice experience, the existing refining agents for casting aluminum alloys still have one or more of the following problems: (1) The degassing and slag removal efficiency of the refining agent is still relatively low, which makes it difficult to meet the production requirements of high-clean casting aluminum alloys. (2) The function of the refining agent is single, which makes it difficult to meet the production requirements of high-performance casting aluminum alloys. (3) During the use of the refining agent, a large amount of irritating smoke is emitted, and the slag-aluminum separation effect is poor, causing serious environmental pollution. Therefore, the existing refining agents for casting aluminum alloys and their preparation methods still need to be improved and developed. Summary of the invention

[0007] In view of the problems mentioned in the background technology, the purpose of the present invention is to provide a composite refining agent for casting aluminum alloy and a preparation method thereof, which can improve the degassing and slag removal efficiency of the refining agent, reduce the gas and slag content of the casting aluminum alloy, refine the modified α-Al grains, Si phase and Fe-rich phase, improve the cleanliness and mechanical properties of the casting aluminum alloy, reduce the emission of irritating smoke and aluminum slag, and solve the problems raised in the background technology by optimizing the component composition and preparation method of the refining agent.

[0008] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows:

[0009] The first aspect of the present invention provides a composite refining agent for casting aluminum alloy, characterized in that the composite refining agent consists of the following components in mass percentage: NaCl 34-36%, NaF 18-22%, TiCl315-17%, SrSO4 8-12%, KPO3 9-13%, and Na2B4O7 6-8%.

[0010] Among them, NaCl is the main component of the composite refining agent. NaCl reacts with aluminum liquid to generate AlCl3 with a boiling point of only 180°C. AlCl3 has a very high vapor pressure and is gaseous in the aluminum liquid. During the floating process, AlCl3 bubbles absorb and capture inclusions and hydrogen in the aluminum liquid, and then escape from the aluminum liquid together, thereby removing slag and hydrogen.

[0011] The main function of NaF is to adsorb and dissolve inclusions such as alumina. NaF molten salt can first destroy the alumina film, dissolve alumina, and dissolve inclusions such as alumina into the molten salt, thus playing a role in removing slag. Secondly, it can reduce the wettability of the interface between inclusions and aluminum liquid, increase the surface tension between inclusions and aluminum liquid, promote the separation of inclusions such as alumina from aluminum liquid, and enhance the slag removal function of the composite refining agent.

[0012] The Ti element generated by the reaction of TiCl3 and aluminum liquid directly enters the aluminum liquid, plays a role in heterogeneous nucleation core organization during the solidification process of aluminum alloy, refines the α-Al grains of aluminum alloy, and transforms the α-Al grains from coarse dendrites to nearly spherical or equiaxed shapes, thereby improving the fluidity, strength and plasticity of cast aluminum alloy. The AlCl3 bubbles generated by the reaction can also absorb and capture inclusions and hydrogen in the aluminum liquid during the floating process, enhancing the slag and hydrogen removal capabilities of the composite refining agent.

[0013] The Sr element generated by the reaction of SrSO4 with aluminum liquid enters the aluminum liquid, which plays a role in refining the modified eutectic Si phase, transforming the eutectic Si phase from coarse needles to fine particles or fibers, eliminating the harm of coarse eutectic Si phase to the strength and plasticity of cast aluminum alloy, and improving the strength and plasticity of cast aluminum alloy. The SO2 bubbles obtained by the reaction can also absorb and capture inclusions and hydrogen in the aluminum liquid during the floating process, enhancing the slag and hydrogen removal capabilities of the composite refining agent.

[0014] KPO3 reacts with aluminum liquid to generate P element which enters into aluminum liquid and can refine the primary Si phase in cast aluminum alloy. For hypereutectic cast aluminum alloy, in addition to the eutectic Si phase, there are also coarse block or lath-shaped primary Si phase. P element can refine the coarse primary Si phase and transform the coarse block or lath-shaped primary Si phase into fine dispersed particles, which can not only improve the strength and plasticity of cast aluminum alloy, but also enhance the wear resistance of cast aluminum alloy.

[0015] The main function of Na2B4O7 is to refine the Fe-rich phase in the modified cast aluminum alloy. Fe is an inevitable impurity element in cast aluminum alloy, usually existing in the form of coarse needle-shaped or flaky Fe-rich phases such as Al3Fe and FeSiAl3, which will damage the strength and plasticity of cast aluminum alloy. Na2B4O7 reacts with aluminum liquid to generate B element and enters the aluminum liquid, which can transform the coarse needle-shaped or flaky Fe-rich phase into fine dispersed particles, eliminate the harm of coarse Fe-rich phase to the strength and plasticity of cast aluminum alloy, and improve the strength and plasticity of cast aluminum alloy.

[0016] The second aspect of the present invention provides a method for preparing a composite refining agent for casting aluminum alloy, characterized in that it comprises the following steps in sequence:

[0017] Step 1: According to the composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 are selected as raw materials for batching;

[0018] Step 2: adding the ingredients into hot water and stirring to dissolve into an aqueous solution, and then heating and evaporating the aqueous solution to obtain a solid crystal;

[0019] Step 3: crushing the solid crystals into particles with a particle size of less than 2 mm, drying and dehydrating the particles to obtain the composite refining agent.

[0020] Preferably, the purity of NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 in step 1 is not less than 99.8%. The raw materials can be industrial products, industrial by-products, or naturally occurring minerals, but the purity of the raw materials must be guaranteed and they cannot contain too many impurities, otherwise it will affect the effect of the composite refining agent and cause secondary pollution to the cast aluminum alloy.

[0021] Preferably, the temperature of the hot water in step 2 is not less than 50° C., the mass ratio of hot water to ingredients is 1-1.5, and the temperature of the aqueous solution during heating and evaporation is 100° C. Too little hot water or too low a temperature will make it difficult to stir and dissolve the ingredients into an aqueous solution, while too much hot water will lead to a long heating and evaporation time, increasing energy consumption and production costs.

[0022] Preferably, the drying and dehydration temperature in step 3 is 150-180°C, and the drying and dehydration time is 3-5 hours. If the temperature is too low or the time is too short, the dehydration will not be thorough. The temperature should not be too high, otherwise the ingredients will decompose and lose their effect. After drying and dehydration, packaging and sealing should be carried out as soon as possible to avoid moisture absorption.

[0023] The third aspect of the present invention also provides a method for using a composite refining agent for casting aluminum alloys, characterized in that the amount of the composite refining agent used is 0.1-0.2% of the weight of the casting aluminum alloy.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The composite refining agent of the present invention has a lower melting point and a more excellent degassing and slag removal effect. The conventional preparation method of the existing refining agent is to mechanically crush the chloride salt and the fluoride salt and then directly mix them to obtain the refining agent. The refining agent prepared by this method has components that exist independently of each other, and there is a lack of synergistic promotion between the components during the refining process, which ultimately leads to a high melting point of the refining agent and a low degassing and slag removal efficiency. The present invention breaks through the tradition and adopts a solution evaporation method to prepare a composite refining agent. Through solution evaporation, the components are re-solidified and recrystallized to form a eutectic with a lower melting point. For example, the melting point of NaCl is usually 801°C, and the melting point of NaF is usually 993°C. When the two form a NaCl·NaF eutectic, the melting point drops to 698°C, thereby greatly reducing the melting point of the composite refining agent, making the composite refining agent easier to dissolve in the cast aluminum alloy liquid, and producing a more excellent degassing and slag removal effect.

[0026] (2) The composite refining agent of the present invention has the dual functions of refining and purification and refining and modification. Existing casting aluminum alloy refining agents usually only contain NaCl, KCl, NaF, CaF, C2Cl6 and other components. Although they have the function of degassing and slag removal, they lack the function of refining and modifying the structure of the casting aluminum alloy. In order to refine and modify the casting aluminum alloy, it is necessary to add a refining and modifying agent, which not only increases the production cost but also increases the production process. In addition to the conventional NaCl and NaF, the composite refining agent of the present invention also contains TiCl3, SrSO4, KPO3, and Na2B4O7. These components not only increase the degassing and slag removal functions of the composite refining agent, but also release trace amounts of Ti, Sr, P, and B elements into the casting aluminum alloy liquid, and respectively refine and modify α-Al grains, eutectic Si phase, primary Si phase and Fe-rich phase during the solidification process, which can eliminate the harm of coarse α-Al grains, eutectic Si phase, primary Si phase and Fe-rich phase to the mechanical properties of the casting aluminum alloy, and improve the strength and plasticity of the casting aluminum alloy.

[0027] (3) The use of the composite refining agent of the present invention is more environmentally friendly and has lower production costs. Existing refining agents mainly contain chloride salts and fluoride salts such as NaCl, KCl, NaF, CaF, C2Cl6 as main components. During use, a large amount of irritating and unpleasant smoke and corrosive gases will be generated, which seriously pollute the environment and endanger the health of workers. Due to the low efficiency of degassing and slag removal of existing refining agents, in order to obtain a cleaner cast aluminum alloy, the amount of refining agent has to be increased. The amount of refining agent usually accounts for 0.3-0.5% of the weight of the cast aluminum alloy liquid. However, increasing the amount of refining agent will increase production costs, increase the emission of aluminum slag, cause more serious environmental pollution, and also cause the content of alkali metal elements such as Na, Ca, K in the cast aluminum alloy to exceed the standard, deteriorating the mechanical properties of the cast aluminum alloy. The composite refining agent of the present invention reduces the content of fluorine salt and chloride salt, can reduce the emission of smoke, has higher degassing and slag removal efficiency, and thus can reduce the amount of composite refining agent used, can not only obtain highly clean cast aluminum alloy, but also reduce the emission of aluminum slag, avoid excessive content of alkali metals such as Na, Ca, K in the cast aluminum alloy, and thus is more environmentally friendly to use, is also conducive to reducing production costs, and enhances the market competitiveness of cast aluminum alloy products. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The invention will be further described below in conjunction with the accompanying drawings.

[0029] Figure 1 The microstructure of the cast aluminum alloy ingot after refining using the composite refining agent of Example 1.

[0030] Figure 2 The microstructure of the cast aluminum alloy ingot after refining using the commercially available conventional refining agent of Comparative Example 2. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] The composite refining agent for casting aluminum alloy is composed of the following components in mass percentage: NaCl 35.12%, NaF19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method of the composite refining agent comprises the following steps in sequence: Step 1: According to the component composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of 99.8% are selected as raw materials for batching; Step 2: Add the ingredients into 70°C hot water, stir and dissolve them into an aqueous solution, the mass ratio of hot water to the ingredients is 1.2, and then heat the aqueous solution to 100°C for evaporation to obtain solid crystals; Step 3: Crush the solid crystals into particles with a particle size of less than 2 mm, dry and dehydrate the particles at 160°C for 4 hours to obtain the composite refining agent.

[0034] Example 2

[0035] The composite refining agent for casting aluminum alloy is composed of the following components in mass percentage: NaCl 34.03%, NaF21.96%, TiCl3 15.03%, SrSO4 11.79%, KPO3 9.22%, and Na2B4O7 7.97%. The preparation method of the composite refining agent comprises the following steps in sequence: Step 1: According to the component composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of 99.8% are selected as raw materials for batching; Step 2: Add the ingredients into 50°C hot water, stir and dissolve them into an aqueous solution, the mass ratio of hot water to the ingredients is 1.5, and then heat the aqueous solution to 100°C for evaporation to obtain solid crystals; Step 3: Crush the solid crystals into particles with a particle size of less than 2 mm, dry and dehydrate the particles at 180°C for 3 hours to obtain the composite refining agent.

[0036] Example 3

[0037] The composite refining agent for casting aluminum alloy is composed of the following components in mass percentage: NaCl 35.95%, NaF19.01%, TiCl3 16.97%, SrSO4 9.03%, KPO3 12.85%, and Na2B4O7 6.19%. The preparation method of the composite refining agent comprises the following steps in sequence: Step 1: According to the component composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of 99.8% are selected as raw materials for batching; Step 2: Add the ingredients into 90°C hot water, stir and dissolve them into an aqueous solution, the mass ratio of hot water to the ingredients is 1, and then heat the aqueous solution to 100°C for evaporation to obtain solid crystals; Step 3: Crush the solid crystals into particles with a particle size of less than 2 mm, dry and dehydrate the particles at 150°C for 5 hours to obtain the composite refining agent.

[0038] Comparative Example 1

[0039] The composite refining agent for casting aluminum alloy is composed of the following components in mass percentage: NaCl 35.12%, NaF19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method of the composite refining agent comprises the following steps in sequence: Step 1: According to the component composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of 99.8% are selected as raw materials for batching; Step 2: Crushing the ingredients into particles with a particle size of less than 2 mm, drying and dehydrating the particles at 160°C for 4 hours to obtain the composite refining agent.

[0040] Comparative Example 2

[0041] The casting aluminum alloy refining agent currently on the market is composed of the following components in mass percentage: NaCl 36.13%, KCl 15.42%, CaF2 16.84%, NaF 19.24%, C2Cl6 12.37%. The refining agent is obtained by directly crushing and mixing the raw materials after drying and dehydration.

[0042] Verification Example 1

[0043] The melting points of the composite refining agent of Example 1, the composite refining agent of Comparative Example 1 and the refining agent of Comparative Example 2 were respectively detected by using an OXFORD-DSC500 differential scanning calorimeter, and the results are shown in Table 1. As can be seen from Table 1, the melting point of the composite refining agent of Example 1 is significantly lower than the melting points of the refining agents of Comparative Example 1 and Comparative Example 2, indicating that the composite refining agent of the present invention has a lower melting point and is more easily dissolved in the casting aluminum alloy liquid, which is not only beneficial to lowering the refining temperature of the casting aluminum alloy liquid and reducing the oxidation and burning loss of the aluminum liquid, but also more conducive to exerting the degassing and slag removal function of the composite refining agent and improving the degassing and slag removal efficiency.

[0044] Table 1 Melting point of refining agent

[0045] Example 1 Comparative Example 1 Comparative Example 2 Melting point / ℃ 723 1280 1014

[0046] Verification Example 2

[0047] The refining agents of Examples 1-3 and Comparative Examples 1-2 were used for refining and modification of ADC12 cast aluminum alloy under the same conditions. The experimental furnace was a 20-ton regenerative gas aluminum melting furnace, the weight of the cast aluminum alloy liquid was 20 tons, and the refining agent was sprayed into the cast aluminum alloy liquid using argon gas with a purity of 99.9% as the carrier medium. The temperature of the cast aluminum alloy liquid during refining was 700°C, the refining time was 20 minutes, and the amount of refining agent added was 0.15% of the weight of the cast aluminum alloy liquid. During the experiment, the use of the refining agent was recorded, including the combustion of the cast aluminum alloy liquid, the smoke emission, the smoke smell, the slag-aluminum separation, and the viscosity of the aluminum slag. Finally, the aluminum slag was collected and weighed. The smaller the weight of the aluminum slag, the better the slag-aluminum separation effect of the refining agent. The results are shown in Table 2. As can be seen from Table 2, the composite refining agent prepared in Examples 1-3 has a small emission during refining, a small smoke irritation, slight combustion of aluminum liquid during refining, easy slag-aluminum separation, loose aluminum slag, and a small amount of aluminum slag. The composite refining agent of Comparative Example 1 is not prepared by solution evaporation method, but directly crushed and mixed, so the slag-aluminum separation effect is slightly poor, and the amount of aluminum slag is slightly large. The commercially available conventional refining agent used in Comparative Example 2 has pungent smoke during refining, large emission, serious combustion of molten aluminum, difficulty in separating slag and aluminum, viscous aluminum slag, and large aluminum slag emission. By comparison, it can be seen that the composite refining agent of the present invention is more environmentally friendly when used, and the slag-aluminum separation effect is easier, which is conducive to reducing aluminum loss and aluminum slag emission.

[0048] Table 2 Comparison of refining conditions of refining agents

[0049]

[0050] Verification Example 3

[0051] The hydrogen content and slag content of the cast aluminum alloy liquid in the furnace before and after refining in Example 2 were tested on site using the HDA-V hydrogen meter and the Analyze PoDFA slag meter. The hydrogen content and slag content of the cast aluminum alloy liquid in the furnace before refining were respectively subtracted from the hydrogen content and slag content of the cast aluminum alloy liquid in the furnace after refining, and then divided by the hydrogen content and slag content of the cast aluminum alloy liquid in the furnace before refining to obtain the degassing rate and slag removal rate of the refining agent, respectively. The results are shown in Tables 3 and 4. It can be seen from Tables 3 and 4 that the degassing rate of the composite refining agent of Examples 1-3 reaches more than 57%, and the slag removal rate reaches more than 50%, while the degassing rate of the refining agent of Comparative Example 1 is 50.4%, and the slag removal rate is 45.9%, and the degassing rate of the commercial refining agent of Comparative Example 2 is only 47.8%, and the slag removal rate is only 41.2%. By comparison, it can be seen that the composite refining agent of the present invention has a higher degassing and slag removal efficiency.

[0052] Table 3 Hydrogen content of cast aluminum alloy liquid before and after refining and degassing rate of refining agent

[0053]

[0054] Table 4 Slag content of cast aluminum alloy liquid before and after refining and slag removal rate of refining agent

[0055]

[0056] Verification Example 4

[0057] The microstructures of the cast aluminum alloy ingots refined by the composite refining agent of Example 1 and the commercial refining agent of Comparative Example 2 were tested, and the results were as follows: Figure 1 and Figure 2 As shown. Figure 1 It can be seen that after refining with the composite refining agent of the present invention, the grain structure of the cast aluminum alloy ingot is fine and uniform, and there are no coarse dendritic α-Al grains, needle-like Si phases and Fe-rich phases. Figure 2 It can be seen that after refining with the conventional refining agent available on the market, the grain structure of the cast aluminum alloy ingot is coarse, the α-Al grains are coarse dendrites, and the Si phase and the Fe-rich phase are coarse needles or laths. By comparison, it can be seen that the composite refining agent of the present invention has an obvious refining and modification effect on the α-Al grains, Si phase and Fe-rich phase of the cast aluminum alloy.

[0058] Verification Example 5

[0059] The casting aluminum alloy liquid in the furnace after refining in Verification Example 2 was sampled and cast into casting aluminum alloy ingots, and the tensile mechanical properties of the casting aluminum alloy ingots were tested, and the results are shown in Table 5. As can be seen from Table 5, the casting aluminum alloy liquid was refined by the composite refining agent prepared in Examples 1-3, and the strength and plasticity of the casting aluminum alloy were significantly higher than those of the casting aluminum alloys refined by the refining agents in Comparative Examples 1 and 2, indicating that the casting aluminum alloy liquid was refined by the composite refining agent of the present invention, by greatly improving the cleanliness of the casting aluminum alloy, refining the metamorphosed coarse α-Al grains, Si phase and Fe-rich phase, and finally significantly improving the strength and plasticity of the casting aluminum alloy.

[0060] Table 5 Tensile mechanical properties of refining cast aluminum alloy

[0061]

Claims

1. A composite refining agent for casting aluminum alloy, characterized in that: The composite refining agent consists of the following components in mass percentage: NaCl 34-36%, NaF 18-22%, TiCl3 15-17%, SrSO4 8-12%, KPO3 9-13%, and Na2B4O7 6-8%.

2. The composite refining agent for casting aluminum alloy according to claim 1, characterized in that: The composite refining agent consists of the following components in percentage by mass: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%.

3. A method for preparing a composite refining agent for casting aluminum alloys, used for preparing the composite refining agent for casting aluminum alloys according to claims 1 and 2, characterized in that: The following steps are included in sequence: Step 1: According to the composition and mass percentage of the composite refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 are selected as raw materials for batching; Step 2: adding the ingredients into hot water and stirring to dissolve into an aqueous solution, and then heating and evaporating the aqueous solution to obtain a solid crystal; Step 3: crushing the solid crystals into particles with a particle size of less than 2 mm, drying and dehydrating the particles to obtain the composite refining agent.

4. The method for preparing the composite refining agent for casting aluminum alloy according to claim 3, characterized in that: The purity of NaCl, NaF, TiCl3, SrSO4, KPO3 and Na2B4O7 in step 1 is not less than 99.8%.

5. The method for preparing the composite refining agent for casting aluminum alloy according to claim 3, characterized in that: The temperature of the hot water in step 2 is not less than 50°C, the mass ratio of hot water to ingredients is 1-1.5, and the temperature of the aqueous solution during heating and evaporation is 100°C.

6. The method for preparing the composite refining agent for casting aluminum alloy according to claim 3, characterized in that: The drying and dehydration temperature in step 3 is 150-180° C., and the drying and dehydration time is 3-5 hours.

7. A method for using the composite refining agent for casting aluminum alloy according to any one of claims 1 to 6, characterized in that: The amount of the composite refining agent used is 0.1-0.2% of the weight of the cast aluminum alloy.

Citation Information

Patent Citations

  • Strontium salt modifier

    CN102127651A

  • Molten aluminium alloy refining agent and preparation method thereof

    CN102409193A

  • Covering agent and aluminium-silicon alloy melt processing method

    CN103820667A

  • Silicon aluminum alloy refining modificator, preparation method of silicon aluminum alloy refining modificator, preparation method of die-casting silicon aluminum alloy and prepared die-casting silicon aluminum alloy

    CN106811614A

  • High-Zn die-casting aluminum alloy and preparation method thereof

    CN109457153A

Cited By

  • Refining agent for electrical aluminum alloy liquid and preparation method thereof

    CN115992313A