Method for remelting casting residues
Through the comprehensive control method of cast residue recovery and converter smelting, the large spray phenomenon and low yield problems in cast residue rotary furnace smelting are solved, efficient recycling and smelting stability of molten steel is achieved, and safety risks and costs are reduced. .
Patent Information
- Application Number
- CN202411023331.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In steelmaking plants, there are problems such as large spraying, low metal yield and serious furnace lining erosion. The existing technology has failed to effectively solve the treatment methods for casting residue rotary furnace smelting.
The cast residue is recovered by cast residue, re-furnace smelting, converter slag control, gun position control and end point control. The cast residue is recovered through the molten iron tank. After the cast residue is re-dumped into the converter, scrap steel is added first and then molten iron is added, and the double slag method is carried out. , controls the gun position and oxygen flow, combines automated calculations and rapid analyzer results to achieve the stability and composition qualification of converter smelting.
It effectively reduces the loss of molten steel, improves the yield of molten steel, optimizes the casting residue recycling process, reduces safety risks and steelmaking costs, and fills the gap in the converter casting residue reagent smelting method.
Smart Images

Figure CN118957408A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a method for smelting casting slag by recycling. Background Art
[0002] In the actual production of steel mills, casting slag is the slag left in the molten steel tank after the continuous casting machine finishes pouring. Sometimes, the molten steel tank pourer fails to confirm the final state of the molten steel tank, and some molten steel will be left in some tanks, which will be turned into the slag tank along with the slag, causing the loss of molten steel and seriously affecting the consumption of steel materials. In order to reduce this part of the economic loss, it is necessary to recycle the casting slag. There are many difficulties in the recycling of casting slag, the return of casting slag to the furnace, and the converter smelting. The converter smelting is very difficult.
[0003] At present, there are methods for treating foaming in the process of casting slag recovery in the domestic public data, but these methods only explain the method of casting slag recovery, and do not discuss the treatment method of casting slag rotary furnace smelting. The converter uses casting slag for smelting, the slag is active, and it is very easy to have a large spray phenomenon, and the metal recovery rate is extremely low, which will also aggravate the erosion of the furnace lining. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to provide a method for recycling casting slag for smelting, by which the purpose of normal smelting of the converter, qualified temperature and qualified composition can be achieved through recycling casting slag, recycling casting slag for smelting, converter slag making control, gun position control, end point control, etc., thereby realizing stable control of the recycling casting slag for converter smelting.
[0005] The technical solution adopted by the present invention is as follows:
[0006] The present invention provides a method for smelting casting slag by recycling the casting slag, comprising the following steps:
[0007] S1, casting slag recovery: using a hot metal ladle to recover the casting slag, after recovery, the hot metal ladle is placed in a pouring room for iron folding;
[0008] S2, casting slag return to the furnace for smelting; the converter is charged with casting slag tanks, and the loading amount is controlled according to the amount of molten iron converted according to the amount of casting slag recovered. During the loading process, scrap steel must be added first, and then molten iron is added. During the process of adding molten iron, the furnace must be shaken back and forth to mix the casting slag and molten iron evenly;
[0009] S3, converter slag control: add casting slag to the furnace, the converter adopts double slag method, according to the different recovery amount of casting slag, the slag material into the converter is appropriately reduced during the converter smelting operation;
[0010] S4, converter gun position control; before double slag, the gun position is low first and then high, and after double slag, the gun position is high, and after stabilization, it is converted to the conventional control model;
[0011] S5, converter endpoint control: according to the steelmaking automation calculation, combined with the furnace mouth flame, use the auxiliary gun to measure TSC, according to the TSC measurement results, blow to the target composition and target temperature of the molten steel, then lift the gun, and quickly tap the steel according to the results of the molten steel rapid analyzer.
[0012] Furthermore, the step S1 specifically includes: using a molten iron ladle to recover the casting slag, the molten iron ladle must have molten iron covering the bottom of the ladle, and the molten iron amount is required to be 30t-80t; placing the prepared molten iron ladle on a cross-over trolley, driving it until the ladle is tipped over, lifting the molten iron ladle to the tipping position by a crane, and after the casting slag is recovered, lifting the molten iron ladle to the cross-over trolley, driving it until the converter is tipped over, and then lifting the molten iron ladle to the ladle room for folding iron.
[0013] Furthermore, the molten iron ladle for recovering the casting slag must be a ladle for calming steelmaking or good top slag modification, and the process from recovering the casting slag in the molten iron ladle to returning the molten iron ladle to the pouring room for folding iron is controlled within 0.5-2 hours, and the maximum number of recovery ladle is 6 ladles.
[0014] Furthermore, the iron folding process specifically includes: when the molten iron tank is transferred back, first check whether the slag surface of the molten iron tank is crusted. If the molten iron tank is crusted, the iron folding can be carried out after processing; when the iron folding weight reaches 50% of the planned weight, stop the iron folding, check the slag surface of the molten iron tank, and after confirming that there is no abnormality, proceed to the next step of iron folding. When the folded iron weight reaches 90% of the planned weight, stop again, confirm the status of the molten iron tank, and after confirming that there is no abnormality, fold the remaining molten iron; after the molten iron tank recovers the casting slag, no desulfurization treatment and slag removal treatment are carried out in the two furnaces. The molten iron tank recovers the casting slag and can only provide LF straight steel grade in the two furnaces.
[0015] Further, the step S2 specifically includes: adding the casting slag tank into the converter, and the loading amount is controlled by converting the molten iron amount according to the amount of casting slag recovery; after the casting slag is recovered, it is converted into iron and added to the converter, and the weight is 20t-25t. If the weight is too large, it means that there is a lot of residual steel in the continuous casting machine. The molten iron conversion method is:
[0016] Casting slag recovery amount: <20t, molten iron conversion amount: 50% recovery rate, that is, actual amount * 0.5; Casting slag recovery amount: 20-25t, molten iron conversion amount: 60% recovery rate, that is, actual amount * 0.6; Casting slag recovery amount: >25t, molten iron conversion amount: 25 * 0.6 + (actual amount - 25);
[0017] During the loading process of the converter, scrap steel must be added first and then molten iron. Since the molten iron tank contains casting slag, iron must be added in small streams. After adding 80t-100t, the converter is shaken back and forth. After there is no abnormal reaction, the remaining molten iron is added. After the molten iron is added, the converter is shaken back and forth twice. Only after there is no violent reaction can the gun be lowered to blow oxygen.
[0018] Furthermore, the step S3 specifically includes: adding casting slag heats, the converter adopts the double slag method, and according to the different amounts of casting slag recovery, the slag material fed into the converter should be appropriately reduced during the converter smelting operation, as follows:
[0019] If the amount of casting slag recovered is less than 20t, the amount of converter lime will be reduced by 1000kg; if the amount of casting slag recovered is 20-25t, the amount of converter lime will be reduced by 1500kg; if the amount of casting slag recovered is greater than 25t, the amount of converter lime will be reduced by 2000kg;
[0020] Slag material addition control: Slag materials mainly supplement CaO, MgO, and slag volume. The added slag materials include active lime, light-burned dolomite and iron ore. The specific method is:
[0021] Control of slag before slag discharge: active lime addition amount is 10±0.5kg / t; lightly burned dolomite addition amount is 15±0.5kg / t; add after 30-40s of blowing;
[0022] Control of slag after slag discharge: when the amount of casting slag recovery is less than 20t, the amount of converter lime reduction is 21±0.5kg / t; when the amount of casting slag recovery is 20-25t, the amount of converter lime reduction is 19±0.5kg / t; when the amount of casting slag recovery is greater than 25t, the amount of converter lime reduction is 17±0.5kg / t; the amount of light-burned dolomite added is 5±0.5kg / t; after slag discharge, add it after the lower gun is ignited; iron ore is added according to the rich temperature after the slag is stable.
[0023] Furthermore, the step S4 specifically includes:
[0024] Blowing gun position: 2900mm-3000mm; Blowing oxygen pressure: 1.0Mpa-1.15Mpa; Blowing oxygen flow rate 54000-56000Nm 3 / h; After 60-70s of blowing, the gun position is lowered to 2400-2450mm, after 130-140s of blowing, the gun position is lowered to 2150-2200mm, after 200-210s of blowing, the gun position is raised to 2600-2650mm, after 250-260s of blowing, the gun position is raised to 3200-3250mm, and the gun position is waiting to release the slag according to the slag situation;
[0025] After slag discharge, re-blowing, opening gun position: 3000-3050mm, oxygen flow rate 45000-46000Nm 3 / h; after successful ignition, the gun position is reduced to 2700-2800mm, and the oxygen flow rate is adjusted to 55000-55500Nm 3 / h.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. It reduces the problem of molten steel loss caused by excess steel in the pouring process of the continuous casting machine, reduces the consumption of steel materials, and effectively improves the molten steel recovery rate;
[0028] 2. It fills the gap in the smelting method of converter casting slag;
[0029] 3. The casting slag recovery process has been optimized, reducing the safety risks in the casting slag recovery process;
[0030] 4. Reduce flux consumption and reduce steelmaking process costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a schematic flow chart of a method for smelting casting slag by recycling it into a furnace. DETAILED DESCRIPTION
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] See attached Figure 1 The present invention provides a method for smelting casting slag, which specifically comprises the following steps:
[0034] S1, casting slag recovery;
[0035] Generally, molten iron ladle is used to recover casting slag. The bottom of the molten iron ladle must be covered with molten iron, and the amount of molten iron required is 30t-80t. The prepared molten iron ladle is placed on the cross-over trolley, driven to the tank tipping position, and the molten iron ladle is lifted to the tank tipping position by the overhead crane. After the casting slag is recovered, the molten iron ladle is lifted to the cross-over trolley, driven to the converter, and then lifted to the tank tipping room for folding iron.
[0036] Requirements for recycling casting slag:
[0037] The casting slag recovered in the molten iron ladle must be the one that has been calmly tapped or has had the top slag modified well. The casting slag cannot be recovered from the boiling steel that has been treated with LF to prevent the top slag from being highly oxidizing and prone to splashing during recovery.
[0038] Strictly control the number of casting slag recovery tanks and recovery time. From the start of casting slag recovery in the molten iron tank to the return of the molten iron tank to the tank, the iron folding time should be controlled within 2 hours, and the number of recovery tanks should be no more than 6 tanks, to avoid the formation of crust on the molten iron tank or serious slag leakage during the converter blowing process.
[0039] Iron folding process after recycling:
[0040] When the molten iron ladle is returned, first check whether the slag surface of the molten iron ladle is crusted. If the molten iron ladle is crusted, it can be folded only after it is treated. When folding iron, pay attention to the changes in the slag surface. When the folded iron weight reaches 50% of the planned weight, stop folding iron, check the slag surface of the molten iron ladle, and after confirming that there is no abnormality, proceed to the next step of folding iron. When the folded iron weight reaches 90% of the planned weight, stop again, confirm the status of the molten iron ladle, and after there is no abnormality, fold the remaining molten iron.
[0041] After the molten iron tank recovers the casting slag, no desulfurization treatment and slag removal treatment are carried out in the two furnaces. The molten iron tank recovers the casting slag in the two furnaces and can only give LF direct steel grades.
[0042] S2, casting slag is returned to the furnace for smelting;
[0043] Converter loading system and loading method:
[0044] The converter is charged with casting slag tanks. The loading amount should be controlled according to the amount of molten iron converted from the amount of casting slag recovered. Generally, after 2 hours of casting slag recovery, it is necessary to convert it into iron and charge it into the converter. The weight is generally 20-25t. If the weight is too large, it means that there is a lot of residual steel in the continuous casting machine. The method for converting the amount of molten iron is as follows:
[0045] The amount of casting slag recovery: <20t, the amount of molten iron converted: based on a 50% recovery rate, that is, the actual amount*0.5; the amount of casting slag recovery: 20-25t, the amount of molten iron converted: based on a 60% recovery rate, that is, the actual amount*0.6; the amount of casting slag recovery: >25t, the amount of molten iron converted: 25*0.6+(actual amount-25).
[0046] Loading method: During the loading process of the converter, scrap steel must be added first, and then molten iron. Since the molten iron tank contains casting slag, iron must be added in small streams. After adding 80-100t, the converter should be shaken back and forth. After there is no abnormal reaction, the remaining molten iron can be added. After the molten iron is added, the converter should be shaken back and forth twice. After there is no violent reaction, the oxygen can be blown from the gun.
[0047] S3, converter slag control;
[0048] The casting slag is added to the converter, and the double slag method is adopted.
[0049] When adding casting slag, the converter adopts the double slag method to prevent the active slag from running away and causing production and environmental accidents. There is a large amount of high-basicity slag in the casting slag, which is beneficial to converter smelting; according to the different amount of casting slag recovery, the slag material should be appropriately reduced during the converter smelting operation, as follows:
[0050] If the amount of casting slag recovered is less than 20t, the amount of converter lime will be reduced by 1000kg; if the amount of casting slag recovered is 20-25t, the amount of converter lime will be reduced by 1500kg; if the amount of casting slag recovered is greater than 25t, the amount of converter lime will be reduced by 2000kg;
[0051] Slag material addition control: Slag materials mainly supplement CaO, MgO, and slag volume. The added slag materials include active lime, light-burned dolomite and iron ore. The specific method is:
[0052] Control of slag before slag discharge: active lime addition amount is 10±0.5kg / t; lightly burned dolomite addition amount is 15±0.5kg / t; add after 30-40s of blowing;
[0053] Control of slag after slag discharge: when the amount of casting slag recovery is less than 20t, the amount of converter lime reduction is 21±0.5kg / t; when the amount of casting slag recovery is 20-25t, the amount of converter lime reduction is 19±0.5kg / t; when the amount of casting slag recovery is greater than 25t, the amount of converter lime reduction is 17±0.5kg / t; the amount of light-burned dolomite added is 5±0.5kg / t; after slag discharge, add it after the lower gun is ignited; iron ore is added according to the rich temperature after the slag is stable.
[0054] S4, converter gun position control;
[0055] Blowing gun position: 2900mm-3000mm; Blowing oxygen pressure: 1.0Mpa-1.15Mpa; Blowing oxygen flow rate 54000-56000Nm 3 / h; After 60-70s of blowing, the gun position is lowered to 2400-2450mm, after 130-140s of blowing, the gun position is lowered to 2150-2200mm, after 200-210s of blowing, the gun position is raised to 2600-2650mm, after 250-260s of blowing, the gun position is raised to 3200-3250mm, and the gun position is waiting to release the slag according to the slag situation;
[0056] After slag discharge, re-blow, open the gun position: 3000-3050mm, oxygen flow rate 45000-46000Nm3 / h; after successful ignition, the gun position is reduced to 2700-2800mm, and the oxygen flow rate is adjusted to 55000-55500Nm 3 / h.
[0057] S5, converter endpoint control;
[0058] According to the steelmaking automation calculation and combined with the furnace mouth flame, the auxiliary gun is used to measure TSC. According to the TSC measurement results, the gun is lifted after blowing to the target composition and target temperature of the molten steel. According to the results of the molten steel rapid analyzer, the steel is quickly tapped.
[0059] The present invention will be further described below by specific examples:
[0060] The method for smelting the casting slag in a converter, the process route: casting slag recovery → casting slag smelting → argon station → refining → casting machine, smelting steel grade QB, ladle grade D, turnover time 100min, casting slag recovery amount 28t, converter target steel tapping temperature 1600℃, finished product requirement P≤0.025%; comprising the following steps:
[0061] S1. Casting slag recovery method: the prepared 6# molten iron ladle, weighing 173 tons and containing 43 tons of molten iron, is placed on the cross-over trolley, opened until the ladle collapses, and the molten iron ladle is hoisted to the ladle flipping position by a crane. It takes 1 hour and 50 minutes to recover 5 ladles of casting slag, and the steel grades QB and SPHC are recovered. After recovery, the crane weighs 201 tons and the casting slag is 28 tons. After the casting slag is recovered, the molten iron ladle is hoisted to the cross-over trolley by a crane, opened until the converter collapses, and then the molten iron ladle is hoisted to the ladle flipping room by a crane for folding.
[0062] When the 6# molten iron ladle was transferred back, there was no crust on the slag surface of the molten iron ladle, and the molten iron was folded in the 2# pit of the ladle. When folding the iron, pay attention to the changes in the slag surface. When the folded iron weight reaches 305 tons, stop folding the iron, check the slag surface of the molten iron ladle, and if there is no abnormality, proceed to the next step of folding the iron. When the folded iron weight reaches the planned weight of 382 tons, stop again, confirm the status of the molten iron ladle, and if there is no abnormality, continue folding the iron. The weight after folding the iron is 395t.
[0063] S2. Casting slag recycling and smelting:
[0064] Loading system: The converter is charged with casting slag tanks, and the charging quantity is controlled by converting the amount of molten iron into the amount of casting slag recovery. This tank is charged with 28 tons of casting slag, and the amount of molten iron converted is: 25*0.6+(28-25)=18 tons.
[0065] Loading method: During the loading process of the converter, scrap steel must be added first, and then molten iron. Since the molten iron tank contains casting slag, iron must be added in small streams. After adding 90 tons, the converter should be shaken back and forth. After there is no abnormal reaction, the remaining molten iron can be added. After the molten iron is added, the converter should be shaken back and forth twice. After there is no violent reaction, oxygen can be blown from the gun.
[0066] S3, converter slag control:
[0067] Add casting slag to the furnace, and the converter adopts the double slag method to prevent the active slag from running away, which may cause production and environmental accidents. There is a large amount of high-basicity slag in the casting slag, which is beneficial to converter smelting. According to the different recovery amounts of casting slag, the slag material should be appropriately reduced during converter smelting operation. The recovery amount of casting slag is 28t, and the reduction amount of converter lime is 2000kg;
[0068] After the lower gun is successfully ignited by oxygen blowing, 2580kg of active lime and 4010kg of light-burned dolomite are added after 32 seconds of blowing. After 255S of blowing, the gun is lifted to discharge the slag according to the slag situation; after the slag is discharged, the blowing is restarted, and after the ignition is successfully ignited, 4450kg of active lime and 1310kg of light-burned dolomite are added.
[0069] S4, converter gun position control:
[0070] Blow oxygen from the lower gun, gun position: 2960mm, oxygen pressure: 1.05Mpa, oxygen flow rate 54800Nm3 / h. After ignition is successful, add the first batch of slag after 32 seconds of refining. After 65s of refining, the gun position is lowered to 2420mm, the gun position is raised to 2155mm for 134S of refining, the gun position is raised to 2610mm for 206S of refining, and the gun position is raised to 3222mm for 255S of refining. The gun position is waiting to release the slag according to the slag situation; after releasing the slag, re-blow, the gun position is opened: 3020mm, oxygen flow rate 45050Nm 3 / h. After the ignition is successful, the gun position is raised to 2710mm and the oxygen flow rate is adjusted to 55800Nm 3 / h.
[0071] S5, converter endpoint control:
[0072] According to the automatic calculation, the actual flame situation on site, the oxygen accumulation reaches 10886Nm 3 When the auxiliary gun was used for TSC test, the TSC measurement results showed that the temperature was 1583℃ and the carbon content was 0.42%. 500kg of cooling material ore was added and the blowing was continued for 90s. The gun was lifted after the blowing was completed. The end temperature was 1622℃ and the oxygen value was 438ppm. The fast analyzer test results showed that C=0.055%, P=0.0163%, Mn=0.08%, S=0.036%, which met the steel grade composition requirements and steel was tapped quickly.
[0073] After the steel is produced, it enters the LF furnace. After the LF furnace is treated qualifiedly, it is put into the casting machine for pouring; the casting machine pouring is normal.
[0074] Matters not described in detail in the present invention are all known technologies.
[0075] The embodiments described above are merely descriptions of preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for smelting casting slag, characterized in that: The method comprises the following steps: S1, casting slag recovery: using a hot metal ladle to recover the casting slag, after recovery, the hot metal ladle is placed in a pouring room for folding iron; S2, casting slag return to the furnace for smelting; the converter is charged with casting slag tanks, and the loading amount is controlled according to the amount of molten iron converted according to the amount of casting slag recovered. During the loading process, scrap steel must be added first, and then molten iron is added. During the process of adding molten iron, the furnace must be shaken back and forth to mix the casting slag and molten iron evenly; S3, converter slag control: add casting slag to the furnace, the converter adopts double slag method, according to the different recovery amount of casting slag, the slag material into the converter is appropriately reduced during the converter smelting operation; S4, converter gun position control; before double slag, the gun position is low first and then high, and after double slag, the gun position is high, and after stabilization, it is converted to the conventional control model; S5, converter endpoint control: according to the steelmaking automation calculation, combined with the furnace mouth flame, use the auxiliary gun to measure TSC, according to the TSC measurement results, blow to the target composition and target temperature of the molten steel, then lift the gun, and quickly tap the steel according to the results of the molten steel rapid analyzer.
2. The method for smelting casting slag according to claim 1, characterized in that: The step S1 specifically includes: using a molten iron ladle to recover the casting slag, the molten iron ladle must have molten iron covering the bottom of the ladle, and the molten iron volume is required to be 30t-80t; placing the prepared molten iron ladle on a cross-over trolley, driving it until the ladle is overturned, lifting the molten iron ladle to the overturning position by a crane, and after the casting slag is recovered, lifting the molten iron ladle to the cross-over trolley, driving it until the converter is overturned, and then lifting the molten iron ladle to the ladle room for folding iron.
3. The method for smelting casting slag according to claim 2, characterized in that: The molten iron ladle for recycling the casting slag must be a ladle for calm steelmaking or top slag modification, and the process from recycling the casting slag in the molten iron ladle to returning the molten iron ladle to the pouring room for folding iron is controlled within 0.5-2 hours, and the maximum number of recycling ladles is 6 ladles.
4. The method for smelting casting slag according to claim 3, characterized in that: The iron folding process specifically includes: when the molten iron tank is transferred back, first check whether the slag surface of the molten iron tank is crusted. If the molten iron tank is crusted, the iron folding can be carried out after processing; when the iron folding weight reaches 50% of the planned weight, stop the iron folding, check the slag surface of the molten iron tank, and after confirming that there is no abnormality, proceed to the next step of iron folding, and when the folded iron weight reaches 90% of the planned weight, stop again, confirm the status of the molten iron tank, and after confirming that there is no abnormality, fold the remaining molten iron; after the molten iron tank recovers the casting slag, no desulfurization treatment and slag removal treatment are carried out in the two furnaces, and the molten iron tank recovers the casting slag in the two furnaces and can only provide LF straight steel grades.
5. The method for smelting casting slag according to claim 4, characterized in that: The step S2 specifically includes: adding the casting slag tank into the converter, and the loading amount is controlled by converting the molten iron amount according to the amount of casting slag recovery; after the casting slag is recovered, it is converted into iron and added into the converter, and the weight is 20t-25t. If the weight is too large, it means that there is a lot of residual steel in the continuous casting machine. The molten iron conversion method is: Casting slag recovery amount: <20t, molten iron conversion amount: 50% recovery rate, that is, actual amount * 0.5; Casting slag recovery amount: 20-25t, molten iron conversion amount: 60% recovery rate, that is, actual amount * 0.6; Casting slag recovery amount: >25t, molten iron conversion amount: 25 * 0.6 + (actual amount - 25); During the loading process of the converter, scrap steel must be added first and then molten iron. Since the molten iron tank contains casting slag, iron must be added in small streams. After adding 80t-100t, the converter is shaken back and forth. After there is no abnormal reaction, the remaining molten iron is added. After the molten iron is added, the converter is shaken back and forth twice. Only after there is no violent reaction can the gun be lowered to blow oxygen.
6. The method for smelting casting slag according to claim 5, characterized in that: The step S3 specifically includes: adding casting slag heats, operating the converter using the double slag method, and appropriately reducing the slag material fed into the converter during the converter smelting operation according to the different amounts of casting slag recovery, as follows: If the amount of casting slag recovered is less than 20t, the amount of converter lime will be reduced by 1000kg; if the amount of casting slag recovered is 20-25t, the amount of converter lime will be reduced by 1500kg; if the amount of casting slag recovered is greater than 25t, the amount of converter lime will be reduced by 2000kg; Slag material addition control: Slag materials mainly supplement CaO, MgO, and slag volume. The added slag materials include active lime, light-burned dolomite and iron ore. The specific method is: Control of slag before slag discharge: active lime addition amount is 10±0.5kg / t; lightly burned dolomite addition amount is 15±0.5kg / t; add after 30-40s of blowing; Control of slag after slag discharge: when the amount of casting slag recovery is less than 20t, the amount of converter lime reduction is 21±0.5kg / t; when the amount of casting slag recovery is 20-25t, the amount of converter lime reduction is 19±0.5kg / t; when the amount of casting slag recovery is greater than 25t, the amount of converter lime reduction is 17±0.5kg / t; the amount of light-burned dolomite added is 5±0.5kg / t; after slag discharge, add it after the lower gun is ignited; iron ore is added according to the rich temperature after the slag is stable.
7. The method for smelting casting slag according to claim 6, characterized in that: The step S4 specifically includes: Blowing gun position: 2900mm-3000mm; Blowing oxygen pressure: 1.0Mpa-1.15Mpa; Blowing oxygen flow rate 54000-56000Nm 3 / h; After 60-70s of blowing, the gun position is lowered to 2400-2450mm, after 130-140s of blowing, the gun position is lowered to 2150-2200mm, after 200-210s of blowing, the gun position is raised to 2600-2650mm, after 250-260s of blowing, the gun position is raised to 3200-3250mm, and the gun position is waiting to release the slag according to the slag situation; After slag discharge, re-blowing, opening gun position: 3000-3050mm, oxygen flow rate 45000-46000Nm 3 / h; after successful ignition, the gun position is reduced to 2700-2800mm, and the oxygen flow rate is adjusted to 55000-55500Nm 3 / h.
Citation Information
Patent Citations
Method for heat application of low-alkalinity casting residue in steel-making
CN102994689A
Method for converter smelting of remelted high-silicon molten steel
CN113789425A
Method for directly returning hot casting residues to converter
CN114317870A
Rapid slagging method for converter double-slag smelting
CN114959164A
Method for returning casting residual molten steel to converter for smelting
CN116024399A