Vanadium-nitrogen reinforced wear-resistant steel and preparation method thereof

Through the preparation method of vanadium nitrogen-strengthening wear-resistant steel, the high-nitrogen vanadium nitrogen alloy, metal cerium and deoxidizer combinations are used to optimize the process flow to form high-performance wear-resistant steel, which solves the wear and corrosion of wear-resistant steel in extreme environments. Problem, efficient and environmentally friendly high-performance material preparation has been achieved.

CN118957410APending Publication Date: 2024-11-15JIANGSU QUNDA MASCH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040519.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing wear-resistant steels are prone to wear and corrosion in extreme application environments, resulting in economic losses and safety accidents. At the same time, traditional preparation processes are inefficient, costly and environmentally polluted.

Method used

The impact toughness, corrosion resistance and wear resistance of steel are improved through the synergistic effect of high nitrogen vanadium nitrogen alloy, metal cerium, deoxidant and cover agent, and the impact toughness, corrosion resistance and wear resistance of steel are improved through gradient sintering. The process of vacuum degassing, rolling, quenching and tempering is optimized to form martensite and bainite structures and a titanium nitride layer is deposited on the surface.

Benefits of technology

It has achieved significant improvements in the high impact performance, corrosion resistance and wear resistance of vanadium nitrogen-strengthened wear-resistant steel, which has reduced production costs, conforms to the concept of green manufacturing, extends service life and meets the high-performance needs of different industries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of wear-resistant steel materials, in particular to vanadium-nitrogen reinforced wear-resistant steel and a preparation method thereof. The invention relates to vanadium-nitrogen reinforced wear-resistant steel, which is prepared from the following preparation raw materials in parts by mass: 100 to 120 parts of pig iron, 1800 to 2100 parts of molten iron, 50 to 60 parts of lime, 25 to 30 parts of dolomite, 30 to 36 parts of high-nitrogen vanadium-nitrogen alloy, 0.12 to 0.15 part of metal cerium, 2 to 2.4 parts of deoxidizer and 1 to 1.2 parts of covering agent. The vanadium-nitrogen reinforced wear-resistant steel shows remarkable advantages in the aspects of material performance, production process, environmental adaptability and the like, and a new solution is provided for development of high-performance wear-resistant steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of wear-resistant steel materials, and in particular to a vanadium-nitrogen reinforced wear-resistant steel and a preparation method thereof. Background Art

[0002] Wear-resistant steel is widely used in mining, metallurgy, construction, coal, cement, electricity and other industries. It can be used to manufacture wear-resistant parts such as crusher linings, excavator shovel teeth, conveyor linings, concrete mixer mixing arms, etc. However, in such extreme application environments, a large number of highly wear-resistant steels are still worn or corroded during use every year, causing huge economic losses to the society and frequent safety accidents.

[0003] At present, high-strength, high-corrosion-resistant and high-wear-resistant steels are widely used in construction, bridges, automobiles, machinery manufacturing and other industries. With the development of science and technology, the performance requirements for materials are getting higher and higher. Vanadium-nitrogen alloy, as a high-quality alloy additive, can effectively improve the strength and wear resistance of steel. At the same time, the traditional wear-resistant steel preparation process has problems such as low efficiency, high cost and environmental pollution.

[0004] Therefore, the development of wear-resistant steel with high impact resistance, high corrosion resistance and high wear resistance and its production process has become the research focus in the world's steel materials field. Summary of the invention

[0005] The purpose of the present application is to provide a vanadium-nitrogen strengthened wear-resistant steel and a preparation method thereof in response to the deficiencies of the current technology. The vanadium-nitrogen strengthened wear-resistant steel of the present application has excellent impact resistance, corrosion resistance and wear resistance. At the same time, the preparation method is simple, the production cost is low, and it is green and environmentally friendly, conforming to the concept of green manufacturing, and meeting the customized needs of different industries for high-performance wear-resistant steel.

[0006] In the first aspect, the present application provides a vanadium nitrogen strengthened wear-resistant steel, which adopts the following technical solution: A vanadium-nitrogen reinforced wear-resistant steel comprises the following raw materials, calculated by weight: 100-120 parts of pig iron, 1800-2100 parts of molten iron, 50-60 parts of lime, 25-30 parts of dolomite, 30-36 parts of high-nitrogen vanadium-nitrogen alloy, 0.12-0.15 parts of metal cerium, 2-2.4 parts of deoxidizer and 1-1.2 parts of covering agent.

[0007] By adopting the above technical scheme, pig iron and molten iron: as basic raw materials, provide the basic components of steel and affect the overall performance of the final product. Lime and dolomite: act as flux in the smelting process, help remove impurities such as silicon, phosphorus and sulfur, and improve the quality of steel. High nitrogen vanadium nitrogen alloy: is the key component of this application, and promotes the precipitation of vanadium carbide and vanadium nitride through high nitrogen content, refines grains, and significantly improves the impact toughness and wear resistance of wear-resistant steel. The fine carbonitrides formed by vanadium, carbon and nitrogen can inhibit the austenitization process, and effectively refine particles during quenching and tempering, thereby improving the overall strength and wear resistance of the material. Metal cerium: as a rare earth element, cerium can effectively reduce the sulfur content in steel, improve the high-temperature oxidation resistance and corrosion resistance of the material, and enhance impact toughness at low temperatures. Deoxidizer and covering agent: deoxidizer is used to remove oxygen from the metal, prevent the occurrence of oxidation reaction, and maintain the purity of the metal; covering agent forms a protective layer during the smelting process to prevent atmospheric oxidation and other pollution of the molten metal. Through the synergistic effect of these combinations, vanadium-nitrogen strengthened wear-resistant steel has not only significantly improved its mechanical properties, but its comprehensive performance in wear resistance, corrosion resistance and impact toughness has also been optimized, meeting the needs of different industries for high-performance wear-resistant steel.

[0008] Preferably, the preparation method of the high nitrogen vanadium nitrogen alloy is to mix 100 parts of vanadium pentoxide, 18 parts of graphite, and 5 parts of urea in proportion by mass to form a mixture; then dry-press the mixture to form a spherical blank with a diameter of 20 mm, place the spherical blank in a push plate kiln, and perform gradient sintering at a nitrogen pressure of 1.08 MPa, wherein the gradient sintering is specifically sintering at 1200°C for 3 hours, sintering at 1400°C for 5 hours, sintering at 1500°C for 3 hours, and cooling to room temperature to obtain a high nitrogen vanadium nitrogen alloy.

[0009] By adopting the above technical scheme, the preparation method of high nitrogen vanadium nitrogen alloy involves multiple key steps, each of which has an important impact on the performance of the final product. First, vanadium pentoxide, graphite and urea are mixed in proportion. Vanadium pentoxide is the source of vanadium, graphite provides carbon, and urea is the source of nitrogen. Urea decomposes at high temperature to release nitrogen, which helps to form vanadium nitride in the alloy. The mixture is dry pressed to form a spherical blank. This step ensures close contact between the raw materials, which is conducive to subsequent chemical reactions and material transfer. Gradient sintering: Low temperature stage (1200℃, 3 hours): The main purpose of this stage is to completely decompose urea, gradually release nitrogen, and start a preliminary reduction reaction to reduce vanadium pentoxide to low-valent vanadium oxide. Medium temperature stage (1400℃, 5 hours): In this stage, the nitridation and carburization reactions of vanadium are more complete, forming vanadium nitride and vanadium carbide. At this time, graphite also begins to participate in the reaction and provide carbon elements. High temperature stage (1500℃, 3 hours): High temperature helps to further promote the nitridation and carburization of vanadium, while making the structure of the alloy more uniform and the grain growth more perfect. Cooling: Controlling the cooling process is crucial to maintaining the phase structure and microstructure of the alloy. Rapid cooling helps to fix the phase structure in the high temperature state and prevent unnecessary phase changes. Through the above preparation method, a high nitrogen vanadium nitrogen alloy with excellent mechanical properties, corrosion resistance and thermal stability can be obtained. This alloy is added to wear-resistant steel, and its high nitrogen content is used to promote the precipitation of vanadium carbide and vanadium nitride, refine the grains, and thus improve the impact toughness and wear resistance of the wear-resistant steel. The fine carbonitrides formed by vanadium and carbon and nitrogen can effectively inhibit the austenitization process, and refine the particles during the heat treatment process, further strengthen the matrix, and improve the overall performance of the material. In addition, the addition of rare earth cerium and the synergistic effect of the high nitrogen vanadium nitrogen alloy further enhance the impact toughness, corrosion resistance and wear resistance of the wear-resistant steel, making it a high-performance material that meets different industrial needs.

[0010] Preferably, the deoxidizer is composed of silicon aluminum barium calcium iron, aluminum manganese iron and silicon carbide in a mass ratio of 2:3:5.

[0011] By adopting the above technical scheme, the use of deoxidizer is crucial in the production process of vanadium nitrogen reinforced wear-resistant steel, because it directly affects the purity and final performance of the steel. The deoxidizer in this application is composed of silicon aluminum barium calcium iron, aluminum manganese iron and silicon carbide in a mass ratio of 2:3:5. These components each have their own unique functions, and there is a synergistic effect between them, which jointly optimizes the deoxidation effect and steel performance. Silicon aluminum barium calcium iron: As a deoxidizer, it can effectively react with oxygen in steel to generate stable oxides, thereby reducing the content of oxygen in steel. Improve the purity of steel, reduce non-metallic inclusions, and improve the mechanical properties of steel. Aluminum manganese iron: A strong deoxidizer that can quickly react with dissolved oxygen in steel to form deoxidation products such as aluminum oxide. Aluminum can also combine with nitrogen in steel to form AlN, which plays a role in refining grains. Silicon carbide: Provides a carbon source, which helps to adjust the carbon content in steel to meet the needs of different performance. Silicon carbide itself has a certain reducibility and can be used as an auxiliary deoxidizer. The combination of SiAlBaCaFe, AlMnFe and SiC can be used for deoxidation at different stages and levels, ensuring the maximum removal of oxygen in steel. AlMnFe deoxidizes quickly, while SiAlBaCaFe further deoxidizes deeply, and SiC provides additional deoxidation and carbon source regulation functions on this basis. The reaction products of these deoxidizers can serve as the core of non-metallic inclusions, promote the aggregation and floating of inclusions, and thus be carried away by slag, reduce the number of inclusions in steel, and improve the purity of steel. AlN formed by AlMnFe and other alloying elements in SiAlBaCaFe can form fine precipitates in steel, which can serve as obstacles to grain growth, thereby refining grains and improving the mechanical properties of steel. By rationally proportioning these deoxidizers, the use of expensive raw materials can be reduced and production costs can be reduced while ensuring the deoxidation effect. At the same time, the reaction products of these deoxidizers have little impact on the environment and meet the requirements of green manufacturing. In summary, the combination of silicon aluminum barium calcium iron, aluminum manganese iron and silicon carbide not only has an effective deoxidation function when used alone, but also further improves the deoxidation efficiency through synergistic effect when used in combination, optimizes the microstructure and properties of the steel, and takes cost and environmental factors into consideration at the same time, providing strong support for the production of high-performance vanadium nitrogen reinforced wear-resistant steel.

[0012] Preferably, the covering agent is a LiCl-KCl covering agent, and the mass ratio of LiCl to KCl in the LiCl-KCl covering agent is 2:3.

[0013] Preferably, the chemical composition of the pig iron is: carbon 3.3-3.5wt%, silicon 0.35-0.39wt%, manganese 0.60-0.71wt%, phosphorus 0.075-0.082wt%, sulfur 0.028-0.033wt%, and the rest is iron and inevitable impurities; the chemical composition of the molten iron is: carbon 4.8-5.0wt%, silicon 0.30-0.40wt%, manganese 0.55-0.62wt%, phosphorus 0.080-0.10wt%, sulfur 0.02-0.03wt%, and the rest is iron and inevitable impurities.

[0014] In a second aspect, the present application provides a method for preparing vanadium-nitrogen reinforced wear-resistant steel, which adopts the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned vanadium-nitrogen reinforced wear-resistant steel, comprising the following steps: S61, adding pig iron and molten iron into a converter according to mass fractions, heating to 1480-1510° C., keeping warm for 30-40 minutes, blowing, adding lime and dolomite during blowing, keeping warm for 10-20 minutes, heating to 1570-1590° C., adding high-nitrogen vanadium-nitrogen alloy and metal cerium, keeping warm for 8-12 minutes, heating to 1630-1650° C., adding deoxidizer and covering agent, and deoxidation refining for 20-30 minutes; S62, maintaining the vacuum degree below 67Pa for 10min-20min for vacuum degassing, and then blowing argon to produce steel after breaking the vacuum, with the argon flow rate of 50-55NL / min, and then pouring to obtain a 100mm×100mm steel billet; S63, sending the steel billet into a heating furnace at 1080-1100° C., heating for 60-70 minutes, and then rolling to obtain a rolled steel billet; S64, heat treating the rolled steel billet, sequentially performing a first quenching, a second quenching and a tempering treatment to obtain a tempered steel billet; S65. Place the tempered steel billet in a radio frequency assisted high frequency electric pulse deposition device, deposit titanium nitride on the surface, connect both sides of the tempered steel billet with a radio frequency voltage of 14-15 MHz, and deposit for 90-100 minutes to obtain vanadium nitrogen reinforced wear-resistant steel.

[0015] By adopting the above technical solutions, each step plays a key role in the preparation process of vanadium nitrogen reinforced wear-resistant steel, and by precisely controlling and optimizing these steps, significant improvements in material properties can be achieved. S61: Melting and alloying: By adding pig iron and molten iron to the converter and gradually heating them up, uniform mixing and preheating of the raw materials are achieved. Lime and dolomite are added at appropriate temperatures, which not only helps to remove impurities (such as phosphorus and sulfur), but also helps to form a suitable slag to protect the metal from oxidation. Addition of high-nitrogen vanadium nitrogen alloy and metallic cerium: Adding these alloying elements at higher temperatures ensures that they are fully dissolved and evenly distributed in the molten steel. The addition of high-nitrogen vanadium nitrogen alloy promotes the precipitation of vanadium carbide and vanadium nitride, which helps to refine the grains, while the addition of rare earth cerium improves the desulfurization effect and high-temperature oxidation resistance. S62: Vacuum degassing: Degassing under high vacuum conditions effectively removes gases (such as hydrogen and nitrogen) in the molten steel, reduces internal defects caused by gases, and improves the toughness and consistency of the material. Argon blowing: By blowing in argon, the molten steel is further protected from secondary oxidation, while helping to remove inclusions and purify the molten steel. S63: Heating and rolling: The billet is evenly heated to a suitable temperature in the heating furnace and then rolled. This process not only changes the shape and size of the steel, but also further refines the grains and optimizes the microstructure through physical deformation. S64: Quenching and tempering: Through a precisely controlled heat treatment process, first quenching to form a martensite phase, then tempering to reduce quenching stress, and finally a composite structure of martensite, residual austenite and acicular bainite is obtained. This structure has good hardness and toughness and excellent wear resistance. Secondary quenching: Further refine the grains and improve the wear resistance of the material. S65: Surface treatment, a titanium nitride layer is deposited on the surface of the billet, which significantly improves the hardness and wear resistance of the surface, while enhancing its corrosion resistance. This layer also improves the overall wear resistance and service life of the material. Through the close coordination and optimization of these steps, vanadium nitrogen reinforced wear-resistant steel not only meets high standards in mechanical properties, but its production process also reflects the modern manufacturing concept of high efficiency and environmental protection. Each step contributes to the performance of the final product. From the processing of raw materials to the final surface treatment, each step is indispensable and together constructs the full performance characteristics of this high-performance material.

[0016] Preferably, in step S63, during the rolling process, the starting rolling temperature is 1120-1150°C, the finishing rolling temperature is 1050-1080°C, the final rolling temperature is 930-950°C, and the cooling rate is 4-5°C / min.

[0017] Preferably, in step S64, the process conditions for the first quenching are a temperature of 900-910°C, which is kept for 1-1.3 hours, and then normalized; the process conditions for the second quenching are a temperature of 880-890°C, which is kept for 1-1.3 hours, and then normalized.

[0018] By adopting the above technical solution, the heat treatment in step S64, especially the two quenching treatments, is a crucial link. These treatments not only optimize the microstructure of the material, but also significantly improve its mechanical properties. The first quenching (900-910°C, holding for 1-1.3 hours, normalizing treatment) refines the grains: the quenching treatment at this temperature promotes the formation of martensite, which has an elongated grain structure, which helps to improve the toughness and strength of the material. Normalizing treatment: Normalizing is carried out after quenching, the purpose is to reduce the hardness and brittleness of the material, while improving its mechanical properties such as ductility and machinability. Normalizing treatment at 910°C can ensure that the material has good plasticity while maintaining high strength. The second quenching (880-890°C, holding for 1-1.3 hours, normalizing treatment) further refines the grains: the second quenching is carried out at a slightly lower temperature, which helps to further refine the grains, thereby improving the wear resistance of the material. Optimizing microstructure: The second quenching can further promote the transformation of retained austenite to martensite or bainite, which have better wear resistance and impact resistance. Normalizing treatment: The purpose of normalizing treatment after the first quenching is the same as that of normalizing treatment after the first quenching. Normalizing after the second quenching is also aimed at adjusting the hardness and brittleness of the material to ensure that the final product has excellent comprehensive performance. Synergistic effect of two quenchings: The first quenching is mainly responsible for forming the basic martensitic structure, while the second quenching further optimizes this structure. Through heat treatment at different temperatures, the grains of the material are refined to the greatest extent, thereby significantly improving wear resistance and impact toughness. Synergistic effect of normalizing treatment: The two normalizing treatments ensure that the material still maintains good mechanical properties after high-temperature quenching, avoids excessive hardening and embrittlement, and makes the material more durable in practical applications. In general, the two quenchings in step S64 and the subsequent normalizing treatment are key steps in the preparation process of vanadium nitrogen strengthened wear-resistant steel. By precisely controlling the temperature and time of heat treatment, the material performance is maximized, making it have excellent performance in extremely demanding industrial applications. This meticulous heat treatment process not only improves the performance of wear-resistant steel, but also ensures the high efficiency and environmental protection of the production process, fully meeting the requirements of green manufacturing.

[0019] Preferably, in step S64, the process conditions of the tempering treatment are: keeping the temperature at 240-250° C. for 1-1.5 hours, and then air cooling to room temperature.

[0020] Preferably, in step S65, the RF-assisted high-frequency electric pulse deposition equipment uses a cylindrical pure titanium target as an electrode, the distance between the cylindrical pure titanium target and the steel billet is 5-6 cm, the output voltage is 20-22 V, the output current is 320-400 A, the discharge frequency is 4000-4500 Hz, and the vacuum degree reaches 3×10 -2 -9×10 -2 Pa, nitrogen flow rate 1000 SCCM.

[0021] By adopting the above technical scheme, the radio frequency assisted high-frequency electric pulse deposition equipment can form a uniform and dense titanium nitride layer on the surface of the steel billet, thereby improving the hardness, wear resistance and corrosion resistance of the wear-resistant steel. The cylindrical pure titanium target is used as an electrode to provide a stable titanium ion source to ensure the deposition quality and thickness of the titanium nitride layer. By adjusting parameters such as the output voltage, current, and discharge frequency, the deposition rate and structure of the titanium nitride layer can be controlled to optimize the performance of the wear-resistant steel. Deposition under vacuum conditions can avoid the influence of impurities in the air on the titanium nitride layer and improve the deposition quality. The control of the nitrogen flow rate also has a great influence on the deposition rate and structure of the titanium nitride layer. An appropriate nitrogen flow rate can improve the deposition efficiency while ensuring the quality of the titanium nitride layer. In summary, the radio frequency assisted high-frequency electric pulse deposition equipment plays a key role in the preparation of vanadium nitrogen strengthened wear-resistant steel. By optimizing the deposition parameters and conditions, the performance of the wear-resistant steel can be significantly improved.

[0022] In summary, the beneficial technical effects of this application are: 1. Addition of high nitrogen vanadium nitrogen alloy: By adding high nitrogen vanadium nitrogen alloy to wear-resistant steel, high nitrogen is used to promote the precipitation of vanadium carbide and vanadium nitride, which plays a role in refining grains. This refinement effect significantly improves the impact toughness and wear resistance of wear-resistant steel and extends the service life of the product. In addition, vanadium can form fine carbonitrides with carbon and nitrogen, inhibiting the austenitization process of steel and effectively improving the performance of wear-resistant steel.

[0023] 2. Application of rare earth cerium: The addition of rare earth cerium can reduce the sulfur content in steel, especially when the carbon content increases, which strengthens the desulfurization effect. This makes the wear-resistant steel have good impact toughness at low temperatures, while improving its high-temperature oxidation resistance and corrosion resistance.

[0024] 3. Synergistic effect of rare earth cerium and high nitrogen vanadium nitrogen alloy: The combined use of these two has played a significant synergistic role in improving the impact toughness, corrosion resistance and wear resistance of wear-resistant steel.

[0025] 4. Heat treatment process after rolling: The quenching + tempering process is adopted to eliminate the quenching stress and reduce the brittleness. This process obtains the martensite + residual austenite + needle-shaped bainite structure. The bainite content gradually increases from the surface to the core, the grains are refined, and the distribution is more uniform, thus achieving the best comprehensive performance.

[0026] 5. Application of secondary quenching: Through secondary quenching, the grains are effectively refined and the wear resistance of wear-resistant steel is effectively improved.

[0027] 6. Vacuum deposited titanium nitride layer: Vacuum deposited titanium nitride layer on the surface of the steel billet significantly improves the hardness, wear resistance and corrosion resistance of the wear-resistant steel.

[0028] 7. Green and environmentally friendly preparation method: The whole preparation process is simple, the production cost is low, and it conforms to the concept of green manufacturing, which is beneficial to environmental protection and resource conservation. DETAILED DESCRIPTION

[0029] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] In the following embodiments and preparation examples, 1 part represents 10 g; the covering agent is a LiCl-KCl covering agent, and the mass ratio of LiCl to KCl in the LiCl-KCl covering agent is 2:3; the chemical composition of the pig iron is: carbon 3.4wt%, silicon 0.37wt%, manganese 0.65wt%, phosphorus 0.079wt%, sulfur 0.029wt%, and the rest is iron and inevitable impurities; the chemical composition of the molten iron is: carbon 5.0wt%, silicon 0.35wt%, manganese 0.57wt%, phosphorus 0.09wt%, sulfur 0.025wt%, and the rest is iron and inevitable impurities.

[0031] Preparation Example 1 Preparation of high nitrogen vanadium nitrogen alloy The preparation method of the high nitrogen vanadium nitrogen alloy is as follows: 100 parts of vanadium pentoxide, 18 parts of graphite, and 5 parts of urea are mixed uniformly according to mass fractions to form a mixture; the mixture is then dry-pressed to form a spherical blank with a diameter of 20 mm, the spherical blank is placed in a push plate kiln, and gradient sintering is performed under a nitrogen pressure of 1.08 MPa, wherein the gradient sintering is specifically sintered at 1200° C. for 3 hours, 1400° C. for 5 hours, and 1500° C. for 3 hours, and then cooled to room temperature to obtain the high nitrogen vanadium nitrogen alloy.

[0032] Example 1 A vanadium-nitrogen reinforced wear-resistant steel comprises the following raw materials, measured by weight: 100 parts of pig iron, 1800 parts of molten iron, 50 parts of lime, 25 parts of dolomite, 30 parts of high-nitrogen vanadium-nitrogen alloy, 0.12 parts of metal cerium, 2 parts of deoxidizer, and 1 part of covering agent, wherein the deoxidizer is composed of silicon-aluminum-barium-calcium-iron, aluminum-manganese-iron and silicon carbide in a weight ratio of 2:3:5.

[0033] The method for preparing the above-mentioned vanadium nitrogen reinforced wear-resistant steel comprises the following steps: S61. Add pig iron and molten iron into a converter according to their mass fractions, heat to 1480°C, keep warm for 30 minutes, blow, add lime and dolomite during blowing, keep warm for 10 minutes, heat to 1570°C, add high nitrogen vanadium nitrogen alloy and metal cerium, keep warm for 8 minutes, heat to 1630°C, add deoxidizer and covering agent, and deoxidize and refine for 20 minutes; S62, maintaining the vacuum degree below 67Pa for 10min for vacuum degassing, then blowing argon to produce steel after breaking the vacuum, the argon flow rate is 50NL / min, and then pouring to obtain a 100mm×100mm steel billet; S63, sending the steel billet into a heating furnace at 1080° C., heating for 70 min, and then rolling, wherein the starting rolling temperature is 1120° C., the finishing rolling temperature is 1050° C., the final rolling temperature is 930° C., and the cooling rate is 4° C. / min, to obtain a rolled steel billet; S64, heat-treating the rolled steel billet, sequentially performing a first quenching, wherein the process conditions of the first quenching are a temperature of 900° C. and a heat preservation of 1.3 h, followed by a normalizing treatment; a second quenching, wherein the process conditions of the second quenching are a temperature of 880° C. and a heat preservation of 1.3 h, followed by a normalizing treatment; and a tempering treatment, wherein the process conditions of the tempering treatment are a temperature of 240° C. and a heat preservation of 1.5 h, followed by air cooling to room temperature, to obtain a tempered steel billet; S65, the tempered steel billet is placed in a radio frequency assisted high frequency electric pulse deposition device, titanium nitride is deposited on the surface, and a radio frequency voltage with a frequency of 14 MHz is connected to both sides of the tempered steel billet. A cylindrical pure titanium target is used as an electrode. The distance between the cylindrical pure titanium target and the steel billet is 5 cm. The output voltage is 20 V, the output current is 320 A, the discharge frequency is 4000 Hz, and the vacuum degree reaches 3×10 -2 Pa, nitrogen flow rate 1000 SCCM, deposition time 100 min, and vanadium nitrogen strengthened wear-resistant steel were obtained.

[0034] Example 2 A vanadium-nitrogen reinforced wear-resistant steel comprises the following raw materials, measured by weight: 120 parts of pig iron, 100 parts of molten iron, 60 parts of lime, 30 parts of dolomite, 36 parts of high-nitrogen vanadium-nitrogen alloy, 0.15 parts of metal cerium, 2.4 parts of deoxidizer, and 1.2 parts of covering agent, wherein the deoxidizer is composed of silicon-aluminum-barium-calcium-iron, aluminum-manganese-iron and silicon carbide in a weight ratio of 2:3:5.

[0035] The method for preparing the above-mentioned vanadium nitrogen reinforced wear-resistant steel comprises the following steps: S61. Add pig iron and molten iron into a converter according to their mass fractions, heat to 1510°C, keep warm for 40 minutes, and then blow. Add lime and dolomite during blowing. After keeping warm for 20 minutes, heat to 1590°C, add high nitrogen vanadium nitrogen alloy and metal cerium, keep warm for 12 minutes, heat to 11650°C, add deoxidizer and covering agent, and deoxidize and refine for 30 minutes; S62, maintaining the vacuum degree below 67Pa for 20min for vacuum degassing, then blowing argon to produce steel after breaking the vacuum, the argon flow rate is 55NL / min, and then pouring to obtain a 100mm×100mm steel billet; S63, sending the steel billet into a heating furnace at 1100° C., heating for 60 min, and then rolling, wherein the starting rolling temperature is 1150° C., the finishing rolling temperature is 1080° C., the final rolling temperature is 950° C., and the cooling rate is 5° C. / min, to obtain a rolled steel billet; S64, heat-treating the rolled steel billet, sequentially performing the first quenching, wherein the process conditions of the first quenching are: a temperature of 910° C. and a heat preservation for 1 hour, followed by normalizing; the second quenching, wherein the process conditions of the second quenching are: a temperature of 890° C. and a heat preservation for 1 hour, followed by normalizing; and tempering, wherein the process conditions of the tempering are: a temperature of 250° C. and a heat preservation for 1 hour, followed by air cooling to room temperature, to obtain a tempered steel billet; S65, the tempered steel billet is placed in a radio frequency assisted high frequency electric pulse deposition device, titanium nitride is deposited on the surface, and a radio frequency voltage of 15 MHz is connected to both sides of the tempered steel billet. A cylindrical pure titanium target is used as an electrode. The distance between the cylindrical pure titanium target and the steel billet is 6 cm. The output voltage is 22 V, the output current is 400 A, the discharge frequency is 4500 Hz, and the vacuum degree reaches 9×10 -2 Pa, nitrogen flow rate 1000 SCCM, deposition time 90 min, vanadium nitrogen strengthened wear-resistant steel was obtained.

[0036] Example 3 A vanadium-nitrogen reinforced wear-resistant steel comprises the following raw materials, calculated by weight: 110 parts of pig iron, 1950 parts of molten iron, 55 parts of lime, 28 parts of dolomite, 33 parts of high-nitrogen vanadium-nitrogen alloy, 0.14 parts of metallic cerium, 2.2 parts of deoxidizer, and 1.1 parts of covering agent, wherein the deoxidizer is composed of silicon-aluminum-barium-calcium-iron, aluminum-manganese-iron and silicon carbide in a weight ratio of 2:3:5.

[0037] The method for preparing the above-mentioned vanadium nitrogen reinforced wear-resistant steel comprises the following steps: S61. Add pig iron and molten iron into a converter according to their mass fractions, heat to 1490°C, keep warm for 36 minutes, blow, add lime and dolomite during blowing, keep warm for 15 minutes, heat to 1580°C, add high nitrogen vanadium nitrogen alloy and metal cerium, keep warm for 10 minutes, heat to 1640°C, add deoxidizer and covering agent, and deoxidize and refine for 25 minutes; S62, maintaining the vacuum degree below 67Pa for 15min for vacuum degassing, then blowing argon to produce steel after breaking the vacuum, the argon flow rate is 53NL / min, and then pouring to obtain a 100mm×100mm steel billet; S63, sending the steel billet into a heating furnace at 1090°C, heating for 65 minutes, and then rolling, wherein the starting rolling temperature is 1140°C, the finishing rolling temperature is 1060°C, the final rolling temperature is 940°C, and the cooling rate is 4.5°C / min, to obtain a rolled steel billet; S64, heat treating the rolled steel billet, sequentially performing the first quenching, wherein the process conditions of the first quenching are a temperature of 905°C and a heat preservation of 1.1h, followed by normalizing; the second quenching, wherein the process conditions of the second quenching are a temperature of 885°C and a heat preservation of 1.1h, followed by normalizing; tempering, wherein the process conditions of the tempering are a temperature of 245°C and a heat preservation of 1.2h, followed by air cooling to room temperature, to obtain a tempered steel billet; S65, the tempered steel billet is placed in a radio frequency assisted high frequency electric pulse deposition device, titanium nitride is deposited on the surface, and a radio frequency voltage of 15 MHz is connected to both sides of the tempered steel billet. A cylindrical pure titanium target is used as an electrode. The distance between the cylindrical pure titanium target and the steel billet is 5.5 cm. The output voltage is 21 V, the output current is 350 A, the discharge frequency is 4300 Hz, and the vacuum degree reaches 5×10 -2 Pa, nitrogen flow rate 1000 SCCM, deposition time 93 minutes, and vanadium nitrogen strengthened wear-resistant steel were obtained.

[0038] Comparative Example 1 The same as Example 3, except that no metallic cerium is added to the raw materials.

[0039] Comparative Example 2 The same as Example 3, except that no high nitrogen vanadium nitrogen alloy is added to the raw materials.

[0040] Comparative Example 3 The same as Example 3, except that an equal amount of aluminum vanadium nitrogen alloy produced by Nantong Runfeng Petrochemical Co., Ltd. is used instead of the high nitrogen vanadium nitrogen alloy prepared in this application.

[0041] Comparative Example 4 The same as Example 3, except that in step S64, there is no second quenching process.

[0042] Comparative Example 5 The same as Example 3, except that there is no step S65.

[0043] Comparative Example 6 The same as Example 3, except that the deoxidizer is silicon aluminum barium calcium iron.

[0044] Comparative Example 7 The same as Example 3, except that the deoxidizer is aluminum manganese iron.

[0045] Comparative Example 8 The same as Example 3, except that the deoxidizer is silicon carbide.

[0046] Performance Testing The vanadium nitrogen reinforced wear-resistant steels prepared in Examples 1 to 3 and Comparative Examples 1 to 8 were sampled and tested for performance. The results are shown in Table 1. Impact performance test: According to the national standard GB / T229-2020 "Charpy pendulum impact test method for metal materials", the impact energy test is carried out at -20℃; Wear resistance test: Wear performance test was conducted using an MLG-130 dry rubber wheel abrasive wear tester in accordance with ASTM-G65 standard; Corrosion resistance test: According to the industry standard JB / T7901-2001 "Metal Material Laboratory Uniform Corrosion Full Immersion Corrosion Test", a simulated corrosion environment full immersion corrosion test of wear-resistant steel was conducted. The corrosion solution simulated the water quality composition of the mine, and the solution concentration was Cl - Concentration 5.096g / L, SO4 2- The concentration was 3.87 g / L, the pH was adjusted to 9.0, and the solution was replaced every 7 days; the solution temperature was set to a constant 30°C; and the corrosion test time was 30 days.

[0047] Table 1 Performance test project <![CDATA[Impact performance / KV2 / J]]> Wear loss / g Corrosion rate / μm / year Example 1 84 1.0635 12.6 Example 2 89 1.0498 11.9 Example 3 86 1.0563 12.3 Comparative Example 1 78 1.2632 14.9 Comparative Example 2 72 1.3704 17.7 Comparative Example 3 80 1.1968 15.8 Comparative Example 4 82 1.1363 13.2 Comparative Example 5 75 2.4361 31.3 Comparative Example 6 81 1.1032 12.9 Comparative Example 7 82 1.1167 13.1 Comparative Example 8 81 1.1026 12.8 Analyzing the data in Table 1, we can see that: 1) The vanadium-nitrogen reinforced wear-resistant steel prepared in Examples 1 to 3 has excellent impact resistance, corrosion resistance and wear resistance. At the same time, the preparation method is simple, the production cost is low, and it is green and environmentally friendly, conforms to the concept of green manufacturing, and meets the customized needs of different industries for high-performance wear-resistant steel.

[0048] 2) The comparative analysis of the performance of the vanadium-nitrogen reinforced wear-resistant steels obtained in Example 3 and Comparative Examples 1-2 shows that there is a synergistic effect between rare earth cerium and the high nitrogen vanadium-nitrogen alloy, which can further enhance the impact toughness, corrosion resistance and wear resistance of the wear-resistant steel.

[0049] 3) The performance comparison analysis of the vanadium nitrogen reinforced wear-resistant steel prepared in combination with Example 3 and Comparative Example 3 shows that the high nitrogen vanadium nitrogen alloy prepared in this application with excellent mechanical properties, corrosion resistance and thermal stability is added to the wear-resistant steel, and its high nitrogen content is used to promote the precipitation of vanadium carbide and vanadium nitride, refine the grains, thereby improving the impact toughness and wear resistance of the wear-resistant steel. The fine carbonitrides formed by vanadium and carbon nitrogen can effectively inhibit the austenitization process, and refine the particles during the heat treatment process, further strengthen the matrix, and improve the overall performance of the material. It can be seen from the data that the performance of the wear-resistant steel obtained by adding a high nitrogen vanadium nitrogen alloy is better than that obtained by adding a vanadium nitrogen alloy.

[0050] 4) The comparative analysis of the performance of the vanadium-nitrogen reinforced wear-resistant steels obtained in Example 3 and Comparative Example 4 shows that the second quenching helps to further refine the grains, thereby improving the wear resistance and impact resistance of the material.

[0051] 5) The comparative analysis of the performance of the vanadium-nitrogen reinforced wear-resistant steels obtained in Example 3 and Comparative Example 5 shows that a uniform and dense titanium nitride layer is formed on the surface of the steel billet, which can significantly improve the impact toughness, wear resistance and corrosion resistance of the wear-resistant steel.

[0052] 6) A comparative analysis of the performance of the vanadium nitrogen reinforced wear-resistant steels prepared in Example 3 and Comparative Examples 6 to 8 shows that the deoxidizer is composed of silicon aluminum barium calcium iron, aluminum manganese iron and silicon carbide in a mass ratio of 2:3:5, and there is a synergistic effect between them, which further improves the deoxidation efficiency, optimizes the microstructure and performance of the steel, and takes into account cost and environmental factors, providing strong support for the production of high-performance vanadium nitrogen reinforced wear-resistant steel.

[0053] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A vanadium-nitrogen strengthened wear-resistant steel, characterized in that: The preparation raw materials include the following by weight: 100-120 parts of pig iron, 1800-2100 parts of molten iron, 50-60 parts of lime, 25-30 parts of dolomite, 30-36 parts of high nitrogen vanadium nitrogen alloy, 0.12-0.15 parts of metal cerium, 2-2.4 parts of deoxidizer and 1-1.2 parts of covering agent.

2. The vanadium-nitrogen strengthened wear-resistant steel according to claim 1, characterized in that: The preparation method of the high nitrogen vanadium nitrogen alloy is as follows: 100 parts of vanadium pentoxide, 18 parts of graphite, and 5 parts of urea are mixed uniformly according to mass fractions to form a mixture; the mixture is then dry-pressed to form a spherical blank with a diameter of 20 mm, the spherical blank is placed in a push plate kiln, and gradient sintering is performed under a nitrogen pressure of 1.08 MPa, wherein the gradient sintering is specifically sintered at 1200° C. for 3 hours, 1400° C. for 5 hours, and 1500° C. for 3 hours, and then cooled to room temperature to obtain the high nitrogen vanadium nitrogen alloy.

3. The vanadium-nitrogen strengthened wear-resistant steel according to claim 1, characterized in that: The deoxidizer is composed of silicon aluminum barium calcium iron, aluminum manganese iron and silicon carbide in a mass ratio of 2:3:

5.

4. The vanadium-nitrogen strengthened wear-resistant steel according to claim 1, characterized in that: The covering agent is a LiCl-KCl covering agent, and the mass ratio of LiCl to KCl in the LiCl-KCl covering agent is 2:

3.

5. The vanadium-nitrogen reinforced wear-resistant steel according to claim 1, characterized in that: The chemical composition of the pig iron is: carbon 3.3-3.5wt%, silicon 0.35-0.39wt%, manganese 0.60-0.71wt%, phosphorus 0.075-0.082wt%, sulfur 0.028-0.033wt%, and the rest is iron and inevitable impurities; the chemical composition of the molten iron is: carbon 4.8-5.0wt%, silicon 0.30-0.40wt%, manganese 0.55-0.62wt%, phosphorus 0.080-0.10wt%, sulfur 0.02-0.03wt%, and the rest is iron and inevitable impurities.

6. A method for preparing a vanadium-nitrogen reinforced wear-resistant steel according to any one of claims 1 to 5, characterized in that: The following steps are involved: S61. Add pig iron and molten iron into a converter according to their mass fractions, heat to 1480-1510° C., keep warm for 30-40 minutes, blow, add lime and dolomite during blowing, keep warm for 10-20 minutes, heat to 1570-1590° C., add high nitrogen vanadium nitrogen alloy and metal cerium, keep warm for 8-12 minutes, heat to 1630-1650° C., add deoxidizer and covering agent, and deoxidize and refine for 20-30 minutes; S62, maintaining the vacuum degree below 67Pa for 10min-20min for vacuum degassing, and then blowing argon to produce steel after breaking the vacuum, with the argon flow rate of 50-55NL / min, and then pouring to obtain a 100mm×100mm steel billet; S63, sending the steel billet into a heating furnace at 1080-1100° C., heating for 60-70 minutes, and then rolling to obtain a rolled steel billet; S64, heat treating the rolled steel billet, sequentially performing a first quenching, a second quenching and a tempering treatment to obtain a tempered steel billet; S65. Place the tempered steel billet in a radio frequency assisted high frequency electric pulse deposition device, deposit titanium nitride on the surface, connect both sides of the tempered steel billet with a radio frequency voltage of 14-15 MHz, and deposit for 90-100 minutes to obtain vanadium nitrogen reinforced wear-resistant steel.

7. The method for preparing vanadium-nitrogen reinforced wear-resistant steel according to claim 6, characterized in that: In step S63, during the rolling process, the starting rolling temperature is 1120-1150°C, the finishing rolling temperature is 1050-1080°C, the final rolling temperature is 930-950°C, and the cooling rate is 4-5°C / min.

8. The method for preparing vanadium-nitrogen reinforced wear-resistant steel according to claim 6, characterized in that: In step S64, the process conditions for the first quenching are: a temperature of 900-910°C, keeping warm for 1-1.3 hours, and then normalizing; the process conditions for the second quenching are: a temperature of 880-890°C, keeping warm for 1-1.3 hours, and then normalizing.

9. The method for preparing vanadium-nitrogen reinforced wear-resistant steel according to claim 6, characterized in that: In step S64, the process conditions of the tempering treatment are: keeping the temperature at 240-250°C for 1-1.5 hours, and then cooling to room temperature in air.

10. The method for preparing vanadium-nitrogen reinforced wear-resistant steel according to claim 6, characterized in that: In step S65, the RF-assisted high-frequency electric pulse deposition equipment uses a cylindrical pure titanium target as an electrode, the distance between the cylindrical pure titanium target and the steel billet is 5-6 cm, the output voltage is 20-22 V, the output current is 320-400 A, the discharge frequency is 4000-4500 Hz, and the vacuum degree reaches 3×10 -2 -9×10 -2 Pa, nitrogen flow rate 1000 SCCM.