Super chemical cobalt plating working solution and application thereof

By using cobalt salts, complexing agents and additives in super electroless cobalt plating working fluid, combining the activation layer and super electroless plating filling steps, the poor stability and high cost of cobalt interconnection preparation in the prior art are solved, and the problem of Efficient and environmentally friendly cobalt interconnect wire preparation, with excellent binding force and anti-electromigration performance.

CN118957552APending Publication Date: 2024-11-15HANGZHOU WIN WIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411033734.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing super electroless plating technology has problems of poor stability, high cost, environmental pollution and health hazards in the preparation of cobalt interconnects, especially the deionized water and palladium activation processes used to cause plating defects and side reactions.

Method used

Using a super electroless cobalt plating working liquid containing cobalt salts, complexing agents, stabilizers, dioximes additives and alcohol additives, the activation layer and super electroless cobalt plating filling step combine with a low eutectic solvent and a polyol reducing agent. Avoid side reactions and palladium activation processes to achieve efficient deposition of cobalt interconnects.

Benefits of technology

Effectively control the deposition rate of cobalt ion, ensure the effectiveness and binding force of cobalt filling, reduce costs, avoid environmental pollution and health hazards, and improve the line resistance and electromigration resistance of cobalt interconnects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970557310000091
    Figure BDA0004970557310000091
Patent Text Reader

Abstract

The invention discloses a super chemical cobalt plating working solution which comprises cobalt salt, a complexing agent, a stabilizer, a dioxime additive, an alcohol additive and deionized water. The invention further discloses application of the active layer to preparation of a cobalt interconnection line on a base material. The application comprises the following steps: 1) preparation of an active layer working solution; (2) preparing a super chemical cobalt plating working solution; 3) pretreating the surface of the base material; 4) preparing an activation layer; 5) performing super chemical cobalt plating filling; and (6) post-treatment. The metal nickel activation layer prepared through the method has excellent binding force, corrosion resistance, stable deposition speed and good density, has the effect of a barrier layer, can block diffusion of cobalt interconnection lines and can serve as an activation layer of follow-up super chemical plating cobalt, and therefore the use of a palladium activation technology can be effectively avoided; the cobalt interconnection wire prepared by the method has excellent binding force and corrosion resistance, relatively low wire resistance and excellent electromigration resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of super chemical plating, and in particular to a super chemical cobalt plating working solution and application thereof. Background Art

[0002] At present, the development of semiconductor components is closely related to Moore's Law. People expect the development of semiconductor components to be lower in energy consumption and higher in speed. As the interconnection spacing decreases, the resistance of copper interconnects and the capacitance between interconnects both show an increasing trend, which indirectly leads to an increase in RC delay, and ultimately causes the speed of semiconductor components to decrease. Therefore, reducing RC delay has become a research hotspot in the field of improving the performance of semiconductor components. Among them, R is the resistance of the interconnect, and C is the capacitance between the interconnects; therefore, it has become a trend to use materials with lower resistance than copper to replace it as a new interconnect material.

[0003] At the nanoscale, cobalt has gained attention due to its advantages such as low line resistivity, excellent anti-electromigration performance (electromigration diffusion activation energy is about 1eV), and high proportion of conductive metal in the groove. As Intel disclosed at a press conference earlier: when cobalt is used as an interconnect material in two ultra-thin wiring layers with a distance of 10nm, it is found that electromigration is reduced by 1 / 10 to 1 / 5, and resistivity is reduced by 1 / 2. At present, cobalt interconnects still use the Damascus process. The traditional Damascus process is as follows: first, a dielectric layer is covered on the silicon substrate, and then the grooves and through holes are etched on the dielectric layer. Then, a barrier layer, an adhesion layer and a seed layer are prepared in turn, and super electroplating cobalt is filled on the seed layer. Finally, chemical mechanical polishing (CMP) is used to remove the excess part to make the surface flat and smooth. The technical means used for the preparation of barrier layers, adhesion layers and seed layers are usually chemical vapor deposition (CVD), physical vapor deposition (PVD) and atomic layer deposition (ALD). CVD / PVD / ALD technology not only requires expensive equipment, but also cannot ensure that the inside of the higher trench can be fully covered, and may cause sagging, resulting in the failure of subsequent super electroplating filling. Super chemical plating can deposit metal layers on insulating substrates, thereby reducing process flow and reducing costs. Therefore, research on super chemical plating direct hole filling to achieve interconnection has received widespread attention. However, at present, super chemical plating still has the following defects:

[0004] (1) Deionized water or pure water is used as the solvent system and most of the sodium hypophosphite, dimethylaminoborane, borohydride and hydrazine hydrate are used as reducing agents, which will inevitably lead to the phenomenon of poor stability of the working solution such as precipitation and decomposition, and the reducing agent is easy to react with water to produce hydrogen, resulting in defects such as pinholes on the surface of the coating, affecting the bonding strength, corrosion resistance and other properties; and the by-products such as phosphate and borate produced by the reaction will not only affect the quality of the coating, but also cause indirect environmental pollution due to improper waste liquid treatment;

[0005] (2) The pre-treatment of super chemical plating filling still uses the palladium activation process, which not only causes a sharp increase in costs, but also palladium will cause great harm to the health of operators. Summary of the invention

[0006] The purpose of the present invention is to provide a super chemical cobalt plating working solution and application thereof, so as to solve the deficiencies of the prior art.

[0007] The present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a super chemical cobalt plating working solution, which comprises a cobalt salt, a complexing agent, a stabilizer, a dioxime additive, an alcohol additive and deionized water;

[0009] The cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate;

[0010] The complexing agent is one or more of carboxylic acids and their salts, and the carboxylic acids include glycine, malic acid, lactic acid, citric acid, and tartaric acid;

[0011] The stabilizer includes one or more of isothiourea propanesulfonic acid inner salt, potassium iodate, ammonium molybdate, and S-carboxyethyl isothiourea salt;

[0012] The dioxime additive includes one or more of dimethylglyoxime, furan dioxime, 1,2-cyclohexanedione dioxime, and dichloroethylene dioxime;

[0013] The alcohol additive is one or more of polyols, and the polyols include pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol;

[0014] The cobalt salt content is 10-150 g / l, the complexing agent content is 25-55 g / l, the stabilizer content is 1-5 ppm, the dioxime additive content is 30-75 g / l, the alcohol additive content is 45-80 g / l, and the balance is deionized water.

[0015] The second aspect of the present invention provides the use of the super chemical cobalt plating working solution on a substrate for preparing cobalt interconnects.

[0016] Further, when applied, the following steps are included:

[0017] 1) Preparation of an activation layer working solution: Adding a nickel salt and a pH buffer to a low eutectic solvent and continuously stirring until the solution becomes clear and transparent, thereby obtaining an activation layer working solution; wherein the nickel salt comprises one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite; the pH buffer comprises tetramethylammonium hydroxide or ammonium hydrogen sulfate; the low eutectic solvent is composed of a hydrogen bond acceptor and a hydrogen bond donor in a molar ratio of 1:1 to 15, the hydrogen bond acceptor is one or more of N,N,N-trimethylglycine and its derivatives, choline chloride and its derivatives, tetramethylammonium chloride and its derivatives, the hydrogen bond donor is one or more of a polyol, and the polyol comprises pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol; the nickel salt content is 5 to 100 g / l, the pH buffer content is 1 to 5 g / l, and the balance is the low eutectic solvent;

[0018] 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of the super chemical cobalt plating working solution, dissolve the cobalt salt, complexing agent, stabilizer, dioxime additive, and alcohol additive in deionized water respectively and then mix them to obtain the super chemical cobalt plating working solution;

[0019] 3) Substrate surface pretreatment: the substrate after the grooves and through holes are etched is subjected to degreasing, water washing, acid washing, water washing and dehydration treatment in sequence;

[0020] 4) Preparation of the activation layer: placing the substrate with the surface pre-treated in the activation layer working solution prepared in step 1) for deposition, and then taking it out for washing; wherein the deposition temperature is 35 to 85° C., and the deposition time is 1 to 3 minutes;

[0021] 5) Super chemical cobalt plating filling: first, the pH of the super chemical cobalt plating working solution prepared in step 2) is adjusted to 4.5-7.5, and then the substrate on which the activation layer is deposited is contacted with the aluminum foil, and both are placed in the super chemical cobalt plating working solution for deposition, and then taken out for washing; wherein the deposition temperature is 65-85° C., and the deposition time is 5-120 min;

[0022] 6) Post-treatment: Blow dry or air dry the substrate after super chemical cobalt plating filling.

[0023] Furthermore, the degreasing and defatting solution used for degreasing and defatting in step 3) includes 25-45 g / l ammonia water, 25-40 g / l Na2CO3, 5-30 g / l NaHCO3, 1-5 g / l hexadecyltrimethylammonium bromide, 25-60 g / l Na2SiO3, and the rest is deionized water. When used, the pH of the degreasing and defatting solution is adjusted to 6.5-7.5; the degreasing and defatting temperature is 50-75°C, and the time is 1-5 min;

[0024] The pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C and the time is 10-30s;

[0025] The dehydration treatment is to place the substrate in ethanol and perform ultrasonic treatment at 40 to 55 KHz for 5 to 15 minutes.

[0026] Furthermore, when the degreasing and degreasing solution is used, its pH is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5.

[0027] Furthermore, in step 5), the pH value of the super chemical cobalt plating working solution is adjusted to 4.5-7.5 using dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5.

[0028] Furthermore, in step 6), compressed air or a hair dryer is used for cold air drying, or the mixture is dried naturally.

[0029] Furthermore, the substrate is a substrate used for manufacturing semiconductors, including a silicon substrate covered with a dielectric layer and a dielectric substrate.

[0030] Beneficial effects of the present invention:

[0031] 1. The dioxime additive in the super chemical cobalt plating working solution of the present invention can effectively control the difference in the deposition rate of cobalt ions at the bottom of the hole and the hole mouth area, thereby effectively ensuring the effectiveness of cobalt filling.

[0032] 2. The super chemical cobalt plating working solution of the present invention can control the content of dioxime additives so that cobalt is deposited alternately in a specific columnar form and a flake form during filling, which can effectively ensure its bonding strength with the substrate while ensuring that the overall cobalt filling layer has a certain degree of pliability.

[0033] 3. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate. A metal nickel activation layer is first deposited on the substrate after surface pretreatment, and then super chemical cobalt plating is performed for filling. The process is simple, easy to operate, and low in cost. The preparation of the cobalt interconnects of the present invention can provide a reference for the manufacturing of a new generation of semiconductors.

[0034] 4. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate, and the prepared metal nickel activation layer has excellent bonding strength, corrosion resistance, stable deposition rate, and good density. The metal nickel activation layer not only has the function of a barrier layer to block the diffusion of cobalt interconnects, but also can serve as an activation layer for subsequent super chemical cobalt plating, i.e., cobalt interconnects, thereby effectively avoiding the use of a palladium activation process.

[0035] 5. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate. During the deposition of the metal nickel activation layer, only the action of the polyol reducing agent is used without introducing other impurities, thereby ensuring the purity of the obtained metal nickel activation layer.

[0036] 6. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate. During the deposition of a metal nickel activation layer, the use of a low eutectic solvent makes it easy to recover the activation layer working waste liquid.

[0037] 7. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate. When super chemical cobalt plating filling is performed, cobalt is initially deposited only by the lead plating of aluminum foil and then by the reduction action of polyols. Therefore, no side reaction will occur during the reaction to generate hydrogen, thereby ensuring that the cobalt interconnects have excellent bonding strength and corrosion resistance.

[0038] 8. The super chemical cobalt plating working solution of the present invention is used for preparing cobalt interconnects on a substrate. The prepared cobalt interconnects have lower line resistance and excellent anti-electromigration performance. DETAILED DESCRIPTION

[0039] The present invention is further explained below in conjunction with the examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0040] The ammonia water mentioned below refers to industrial ammonia water, which is an aqueous solution containing 25% to 28% ammonia.

[0041] The crystal water contained in the following compounds is not included in the mass.

[0042] A super chemical cobalt plating working solution comprises 10-150 g / l of cobalt salt, 25-55 g / l of complexing agent, 1-5 ppm of stabilizer, 30-75 g / l of dioxime additives, 45-80 g / l of alcohol additives, and the balance is deionized water. Wherein, the cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate; the complexing agent is one or more of carboxylic acids and their salts, and the carboxylic acids include glycine, malic acid, lactic acid, citric acid, and tartaric acid; the stabilizer includes one or more of isothioureapropanesulfonic acid inner salt, potassium iodate, ammonium molybdate, and S-carboxyethylisothiourea salt; the dioxime additive includes one or more of dimethylglyoxime, furan dioxime, 1,2-cyclohexanedione dioxime, and dichloroethylene dioxime; the alcohol additive is one or more of polyols, and the polyols include pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol.

[0043] The above-mentioned super chemical cobalt plating working solution is used for preparing cobalt interconnects on a substrate, and when used, the following steps are included:

[0044] 1) Preparation of an activation layer working solution: Adding a nickel salt and a pH buffer to a low eutectic solvent and continuously stirring until the solution becomes clear and transparent, thereby obtaining an activation layer working solution; wherein the nickel salt comprises one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite; the pH buffer comprises tetramethylammonium hydroxide or ammonium hydrogen sulfate; the low eutectic solvent is composed of a hydrogen bond acceptor and a hydrogen bond donor in a molar ratio of 1:1 to 15, the hydrogen bond acceptor is one or more of N,N,N-trimethylglycine and its derivatives, choline chloride and its derivatives, tetramethylammonium chloride and its derivatives, the hydrogen bond donor is one or more of a polyol, and the polyol comprises pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol; the nickel salt content is 5 to 100 g / l, the pH buffer content is 1 to 5 g / l, and the balance is the low eutectic solvent;

[0045] 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of the super chemical cobalt plating working solution, dissolve the cobalt salt, complexing agent, stabilizer, dioxime additive, and alcohol additive in deionized water respectively and then mix them to obtain the super chemical cobalt plating working solution;

[0046] 3) Substrate surface pretreatment: The substrate after etching the grooves and through holes is subjected to degreasing, water washing, acid washing, water washing and dehydration treatment in sequence; wherein the degreasing and degreasing solution used for degreasing and degreasing includes 25-45g / l ammonia water, 25-40g / l Na2CO3, 5-30g / l NaHCO3, 1-5g / l hexadecyltrimethylammonium bromide, 25-60g / l Na2SiO3, the rest is deionized water, and when in use, the pH is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid, the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5; the temperature for degreasing and degreasing is 50-75°C, and the time is 1-5min; the pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C, and the time is 10-30s; the dehydration treatment is to place the substrate in ethanol and perform ultrasonic treatment at 40-55KHz for 5-15min;

[0047] 4) Preparation of the activation layer: placing the substrate with the surface pre-treated in the activation layer working solution prepared in step 1) for deposition, and then taking it out for washing; wherein the deposition temperature is 35 to 85° C., and the deposition time is 1 to 3 minutes;

[0048] 5) Super chemical cobalt plating filling: first, the pH value of the super chemical cobalt plating working solution prepared in step 2) is adjusted to 4.5-7.5 using dilute ammonia water or dilute sulfuric acid, and then the substrate on which the activation layer is deposited is contacted with the aluminum foil, and both are placed in the super chemical cobalt plating working solution for deposition, and then taken out for washing; wherein the deposition temperature is 65-85°C, and the deposition time is 5-120 min; wherein the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5;

[0049] 6) Post-treatment: Blow-dry or air-dry the substrate after super chemical cobalt plating for subsequent processes (such as CMP); the blowing includes using compressed air or a hair dryer for cold air drying, and the air drying includes natural drying.

[0050] The substrate mentioned above is a substrate used for manufacturing semiconductors, including a silicon substrate covered with a dielectric layer and a dielectric substrate.

[0051] The adhesion of the parts in the following embodiments is tested by referring to the cross-hatch test in 2.8 Scribe and Cross-hatch Test in GBT5270-2005 "Review of Test Methods for Adhesion Strength of Electrodeposited and Chemically Deposited Metal Coatings on Metal Substrates"; the corrosion resistance is tested by referring to 5.2.2 Neutral Salt Spray Test (NSS) in GBT10125-2021 "Artificial Atmosphere Corrosion Test Salt Spray Test"; the line resistance of the cobalt connecting wire is measured by referring to GBT19248-2003 "Test Method for Package Lead Resistance"; TEM-EDS-Mapping is used to observe whether there is cobalt element in the substrate to indirectly characterize the barrier performance of the barrier layer, and whether there is cobalt element in the barrier layer to indirectly characterize the anti-electromigration performance of the cobalt connecting wire.

[0052] The degreasing and degreasing solution in the following examples consists of 40 g / l ammonia water, 35 g / l Na2CO3, 20 g / l NaHCO3, 4.5 g / l hexadecyltrimethylammonium bromide, 50 / l Na2SiO3 and deionized water, and its pH is adjusted to 7.0 using dilute ammonia water (prepared by mixing ammonia water and deionized water in a volume ratio of 1:1) or dilute sulfuric acid (prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5).

[0053] Example 1

[0054] The composition of the super chemical cobalt plating working solution in this embodiment is as follows: 120 g / l of cobalt sulfate, 15 g / l of glycine, 10 g / l of citric acid, 5 ppm of ammonium molybdate, 30 g / l of 1,2-cyclohexanedione dioxime, 55 g / l of neopentyl glycol and deionized water, and the pH is adjusted to 4.5 with dilute ammonia water (ammonia water and deionized water are mixed in a volume ratio of 1:1) or dilute sulfuric acid (concentrated sulfuric acid and deionized water are mixed in a volume ratio of 1:5).

[0055] The specific operations are as follows:

[0056] 1) Preparation of an activation layer working solution: nickel sulfate and tetramethylammonium hydroxide are added to a low eutectic solvent composed of N,N,N-trimethylglycine and ethylene glycol in a molar ratio of 1:5, with a nickel sulfate content of 80 g / l and a tetramethylammonium hydroxide content of 5 g / l, and the mixture is stirred continuously until the solution becomes clear and transparent to obtain an activation layer working solution;

[0057] 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of the super chemical cobalt plating working solution, dissolve cobalt sulfate, glycine, citric acid, ammonium molybdate, 1,2-cyclohexanedione dioxime, and neopentyl glycol in deionized water respectively and then mix them to obtain the super chemical cobalt plating working solution;

[0058] 3) Substrate surface pretreatment: Place the substrate (silicon substrate covered with a dielectric layer, i.e., a silicon substrate for preparing semiconductors and having completed the semiconductor pre-process) after etching the grooves and through holes in a degreasing and degreasing solution at 70°C and pH 7.0 for degreasing and degreasing for 5 minutes, then rinse with deionized water, then place the substrate in a 25°C hydrochloric acid solution (prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio of 1:1) for pickling for 15 seconds, then rinse with deionized water, and finally place in ethanol for ultrasonic dehydration at 55KHz for 15 minutes for use;

[0059] 4) Preparation of the activation layer: Place the substrate with the pre-treated surface in the activation layer working solution prepared in step 1) at 45° C. for deposition for 3 minutes, then take it out and wash it with deionized water;

[0060] 5) Super chemical cobalt plating filling: The substrate with the above-mentioned deposited activation layer is placed in contact with the aluminum foil, and placed together in a super chemical cobalt plating working solution at 70° C. and pH 4.5 for deposition for 30 minutes, and then taken out and washed with deionized water;

[0061] 6) Post-treatment: Use compressed nitrogen to dry the substrate after super chemical cobalt plating.

[0062] Example 2

[0063] The components of the super chemical cobalt plating working solution in this embodiment are as follows: 120 g / l of cobalt sulfamate, 20 g / l of tartaric acid, 20 g / l of malic acid, 3 ppm of isothioureapropanesulfonic acid inner salt, 30 g / l of dichloroethylenedioxime, 65 g / l of ethylene glycol and deionized water, and the pH is adjusted to 5.0 with dilute ammonia water (prepared by mixing ammonia water and deionized water in a volume ratio of 1:1) or dilute sulfuric acid (prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5).

[0064] The specific operations are as follows:

[0065] 1) Preparation of an activation layer working solution: nickel sulfate and tetramethylammonium hydroxide are added to a low eutectic solvent composed of choline chloride and ethylene glycol in a molar ratio of 1:10, with a nickel sulfate content of 90 g / l and a tetramethylammonium hydroxide content of 5 g / l, and the mixture is stirred continuously until the solution becomes clear and transparent to obtain an activation layer working solution;

[0066] 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of super chemical cobalt plating working solution, dissolve cobalt sulfamate, tartaric acid, malic acid, isothiourea propanesulfonic acid inner salt, dichloroethylene dioxime, and ethylene glycol in deionized water respectively and then mix them to obtain super chemical cobalt plating working solution;

[0067] 3) Substrate surface pretreatment: Place the substrate (silicon substrate covered with a dielectric layer, i.e., a silicon substrate for preparing semiconductors and having completed the semiconductor pre-process) after etching the grooves and through holes in a degreasing and degreasing solution at 70°C and pH 7.0 for degreasing and degreasing for 5 minutes, then rinse with deionized water, then place the substrate in a 25°C hydrochloric acid solution (prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio of 1:1) for pickling for 15 seconds, then rinse with deionized water, and finally place in ethanol for ultrasonic dehydration at 55KHz for 15 minutes for use;

[0068] 4) Preparation of the activation layer: Place the substrate with the pre-treated surface in the activation layer working solution prepared in step 1) at 70° C. for 2 minutes, then take it out and wash it with deionized water;

[0069] 5) Super chemical cobalt plating filling: The substrate with the above-mentioned deposited activation layer is placed in contact with the aluminum foil, and placed together in a super chemical cobalt plating working solution at 70° C. and pH 5.0 for deposition for 30 minutes, and then taken out and washed with deionized water;

[0070] 6) Post-treatment: Use compressed nitrogen to dry the substrate after super chemical cobalt plating.

[0071] Example 3

[0072] The composition of the super chemical cobalt plating working solution in this embodiment is as follows: 100 g / l of cobalt chloride, 20 g / l of tartaric acid, 20 g / l of lactic acid, 3 ppm of isothioureapropanesulfonic acid inner salt, 60 g / l of dimethylglyoxime, 70 g / l of ethylene glycol and deionized water, and the pH is adjusted to 5.0 with dilute ammonia water (prepared by mixing ammonia water and deionized water in a volume ratio of 1:1) or dilute sulfuric acid (prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5).

[0073] The specific operations are as follows:

[0074] 1) Preparation of an activation layer working solution: nickel sulfate and ammonium bisulfate are added to a low eutectic solvent consisting of choline chloride and butanediol in a molar ratio of 1:8, with a nickel sulfate content of 90 g / l and an ammonium bisulfate content of 5 g / l, and the mixture is stirred continuously until the solution becomes clear and transparent to obtain an activation layer working solution;

[0075] 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of super chemical cobalt plating working solution, dissolve cobalt chloride, tartaric acid, lactic acid, isothioureapropanesulfonic acid inner salt, dimethylglyoxime, and ethylene glycol in deionized water respectively and then mix them to obtain super chemical cobalt plating working solution;

[0076] 3) Substrate surface pretreatment: Place the substrate (silicon substrate covered with a dielectric layer, i.e., a silicon substrate for preparing semiconductors and having completed the semiconductor pre-process) after etching the grooves and through holes in a degreasing and degreasing solution at 70°C and pH 7.0 for degreasing and degreasing for 5 minutes, then rinse with deionized water, then place the substrate in a 25°C hydrochloric acid solution (prepared by mixing concentrated hydrochloric acid and deionized water in a volume ratio of 1:1) for pickling for 15 seconds, then rinse with deionized water, and finally place in ethanol for ultrasonic dehydration at 55KHz for 15 minutes for use;

[0077] 4) Preparation of the activation layer: Place the substrate with the pre-treated surface in the activation layer working solution prepared in step 1) at 75° C. for 1 minute of deposition, then take it out and wash it with deionized water;

[0078] 5) Super chemical cobalt plating filling: The substrate with the above-mentioned deposited activation layer is placed in contact with the aluminum foil, and placed together in a super chemical cobalt plating working solution at 80° C. and pH 5.0 for deposition for 25 minutes, and then taken out and washed with deionized water;

[0079] 6) Post-treatment: Use compressed nitrogen to dry the substrate after super chemical cobalt plating.

[0080] The performance of the products obtained in each embodiment was tested, and the test results are shown in Table 1.

[0081] Table 1

[0082]

Claims

1. A super chemical cobalt plating working solution, characterized in that: The super chemical cobalt plating working solution comprises cobalt salt, complexing agent, stabilizer, dioxime additive, alcohol additive and deionized water; The cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate; The complexing agent is one or more of carboxylic acids and their salts, and the carboxylic acids include glycine, malic acid, lactic acid, citric acid, and tartaric acid; The stabilizer includes one or more of isothiourea propanesulfonic acid inner salt, potassium iodate, ammonium molybdate, and S-carboxyethyl isothiourea sulfonic acid salt; The dioxime additive includes one or more of dimethylglyoxime, furan dioxime, 1,2-cyclohexanedione dioxime, and dichloroethylene dioxime; The alcohol additive is one or more of polyols, and the polyols include pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol; The cobalt salt content is 10-150 g / l, the complexing agent content is 25-55 g / l, the stabilizer content is 1-5 ppm, the dioxime additive content is 30-75 g / l, the alcohol additive content is 45-80 g / l, and the balance is deionized water.

2. Use of the super chemical cobalt plating working solution according to claim 1 for preparing cobalt interconnects on a substrate.

3. The use according to claim 2, characterized in that: When applied, the following steps are included: 1) Preparation of an activation layer working solution: Adding a nickel salt and a pH buffer to a low eutectic solvent and continuously stirring until the solution becomes clear and transparent, thereby obtaining an activation layer working solution; wherein the nickel salt comprises one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite; the pH buffer comprises tetramethylammonium hydroxide or ammonium hydrogen sulfate; the low eutectic solvent is composed of a hydrogen bond acceptor and a hydrogen bond donor in a molar ratio of 1:1 to 15, the hydrogen bond acceptor is one or more of N,N,N-trimethylglycine and its derivatives, choline chloride and its derivatives, tetramethylammonium chloride and its derivatives, the hydrogen bond donor is one or more of a polyol, and the polyol comprises pentaerythritol, neopentyl glycol, ethylene glycol, and butanediol; the nickel salt content is 5 to 100 g / l, the pH buffer content is 1 to 5 g / l, and the balance is the low eutectic solvent; 2) Preparation of super chemical cobalt plating working solution: Weigh each component according to the formula of the super chemical cobalt plating working solution, dissolve the cobalt salt, complexing agent, stabilizer, dioxime additive, and alcohol additive in deionized water respectively and then mix them to obtain the super chemical cobalt plating working solution; 3) Substrate surface pretreatment: the substrate after the grooves and through holes are etched is subjected to degreasing, water washing, acid washing, water washing and dehydration treatment in sequence; 4) Preparation of the activation layer: placing the substrate with the surface pre-treated in the activation layer working solution prepared in step 1) for deposition, and then taking it out for washing; wherein the deposition temperature is 35 to 85° C., and the deposition time is 1 to 3 minutes; 5) Super chemical cobalt plating filling: first, the pH of the super chemical cobalt plating working solution prepared in step 2) is adjusted to 4.5-7.5, and then the substrate on which the activation layer is deposited is contacted with the aluminum foil, and both are placed in the super chemical cobalt plating working solution for deposition, and then taken out for washing; wherein the deposition temperature is 65-85° C., and the deposition time is 5-120 min; 6) Post-treatment: Blow dry or air dry the substrate after super chemical cobalt plating filling.

4. The use according to claim 3, characterized in that: The degreasing and degreasing solution used in step 3) comprises 25-45 g / l ammonia water, 25-40 g / l Na2CO3, 5-30 g / l NaHCO3, 1-5 g / l hexadecyltrimethylammonium bromide, 25-60 g / l Na2SiO3, and the rest is deionized water. When used, the pH value of the degreasing and degreasing solution is adjusted to 6.5-7.5; the degreasing and degreasing temperature is 50-75°C, and the time is 1-5 min; The pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C and the time is 10-30s; The dehydration treatment is to place the substrate in ethanol and perform ultrasonic treatment at 40 to 55 KHz for 5 to 15 minutes.

5. The use according to claim 4, characterized in that: When the degreasing and degreasing solution is used, its pH is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:

5.

6. The use according to claim 3, characterized in that: In step 5), the pH value of the super chemical cobalt plating working solution is adjusted to 4.5-7.5 using dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:

5.

7. The use according to claim 3, characterized in that: In step 6), use compressed air or a hair dryer to blow dry with cold air, or let it dry naturally.

8. The use according to any one of claims 2 to 7, characterized in that: The substrate is a substrate used for manufacturing semiconductors, including a silicon substrate covered with a dielectric layer and a dielectric substrate.