Reverse displacement deposition liquid based on deep eutectic solvent and application of reverse displacement deposition liquid in reverse displacement preparation of metal activation layer on copper surface
By using a reverse replacement sediment with a low eutectic solvent system on the copper surface, the poor stability and defects in the preparation of cobalt or nickel metal layers on the copper substrate are solved, and the high binding force and good resistance of cobalt or nickel metal layers are achieved. Corrosiveness, replaces the palladium activation process, reduces costs and simplifies operations.
Patent Information
- Application Number
- CN202411033757.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art When preparing cobalt or nickel metal layers on copper substrates, there are poor stability and defects caused by metal salt precipitation, decomposition and oxidation reactions, which are difficult to replace the palladium activation process, and the standard electrode potential of cobalt or nickel is low, making it difficult to Reverse displacement deposition is achieved.
The metal activated layer is prepared by reverse displacement deposition on the copper surface by reverse displacement deposition on the copper surface using reverse displacement deposition solution, including nickel or cobalt salt, pH buffer, and a low melt solvent composed of hydrogen bond acceptor and hydrogen bond donor. , avoid precipitation and oxidation reaction of metal salts, and realize reverse replacement of cobalt or nickel.
The precipitation and oxidation reaction of metal salts are effectively avoided, and the high binding force, good corrosion resistance and stable deposition speed of the cobalt or nickel metal layer is ensured, which replaces the palladium activation process, reduces costs and simplifies operation.
Smart Images

Figure BDA0004970562990000071 
Figure BDA0004970562990000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical plating activated catalytic layer, and in particular to a reverse displacement deposition liquid based on a low eutectic solvent and an application thereof in preparing a metal activation layer by reverse displacement on a copper surface. Background Art
[0002] In the manufacture of printed circuit boards (PCBs), the copper foil on the circuit board has weak corrosion resistance and is easily oxidized into copper oxide or cuprous oxide. There is no oxidation protection layer that can prevent further oxidation reaction of the copper substrate, which will seriously affect the welding quality. Through surface treatment process, the oxidation of copper foil can be prevented, thereby ensuring excellent solderability and corresponding electrical properties. The immersion gold and nickel-palladium-gold processes can effectively avoid the oxidation of copper foil, and can be used for lead-free soldering, which has great development potential. Both the immersion gold and nickel-palladium-gold process will undergo an activation procedure. The current main activation process is palladium activation. In addition to the high cost and harm to the environment and human health, this activation process is very likely to cause subsequent overflow plating of chemical nickel plating in the actual application process, especially for electronic components PCB. According to records, nickel, cobalt, etc. have certain catalytic activity on sodium hypophosphite, which can induce spontaneous chemical nickel plating on the surface of copper and its alloys. Compared with the palladium activation process, the nickel and cobalt metal activation process not only has cost advantages, but also can effectively avoid subsequent overflow plating.
[0003] The metal replacement reduction precipitation method is an oxidation-reduction process that uses a more negatively charged metal as a reducing agent to replace another more positively charged metal ion from the solution. It has the advantages of simple operation process and low cost. However, due to the standard electrode potential of copper (E Cu2+ / Cu =0.337V) is higher than the standard electrode potential of cobalt (E Co2+ / Co =-0.277V), the standard electrode potential of nickel, so it is difficult to use replacement deposition to prepare cobalt or copper metal layers on the copper surface. Studying a method for depositing nickel and cobalt metal layers on the copper metal surface has very important practical and theoretical significance for realizing the use of nickel and cobalt metal activation process to replace palladium activation process.
[0004] Chinese patents CN114164421A (publication date 2022.03.11), Chinese patents CN110565078A (publication date 2019.12.13), etc. all disclose a method of using reverse displacement deposition to prepare a cobalt or nickel-containing film on a copper substrate. Since both use a water solvent system, even if a large amount of additives such as complexing agents are added to the solvent, a large amount of metal salts will inevitably precipitate, decompose, and have poor stability; and under acidic or alkaline conditions, it is inevitable that metal ions as reducing agents will react with water to produce hydrogen while undergoing an oxidation reaction, resulting in defects such as pinholes on the surface of the metal layer that affect properties such as bonding strength and corrosion resistance.
[0005] A deep eutectic solvent is a new liquid formed by the combination of hydrogen bond acceptors and hydrogen bond donors in a certain stoichiometric ratio and the self-association of the components through hydrogen bonds. The inventors have found that the above-mentioned defects can be effectively avoided when a deep eutectic solvent system is used for reverse displacement deposition. Summary of the invention
[0006] The purpose of the present invention is to provide a reverse displacement deposition solution based on a low eutectic solvent and its application in preparing a metal activation layer by reverse displacement on a copper surface, so as to solve the shortcomings of the prior art.
[0007] The present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a reverse displacement deposition solution based on a deep eutectic solvent, comprising a metal salt, a pH buffer and a deep eutectic solvent;
[0009] The metal salt is a nickel salt or a cobalt salt, wherein the nickel salt includes one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite, and the cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate;
[0010] The pH buffer includes tetramethylammonium hydroxide or ammonium bisulfate;
[0011] The low eutectic solvent is prepared by drying a hydrogen bond acceptor and a hydrogen bond donor respectively, mixing them in a molar ratio of 1:1 to 3, heating, melting, and stirring to form a clear and transparent solvent; the hydrogen bond acceptor includes one or more of betaine, choline chloride, and tetramethylammonium chloride; the hydrogen bond donor includes one or more of polyols, carboxylic acids, amino acids, and urea, the polyols include ethylene glycol and pentaerythritol, the carboxylic acids include tartaric acid and citric acid, and the amino acids include glycine;
[0012] The content of the metal salt is 5 to 180 g / l, the content of the pH buffer is 1 to 20 g / l, and the balance is a low eutectic solvent.
[0013] The second aspect of the present invention provides the use of the above-mentioned reverse displacement deposition solution based on a low eutectic solvent in the preparation of a metal activation layer by reverse displacement on a copper surface, which comprises the following steps:
[0014] (1) Preparation of a low eutectic solvent: The hydrogen bond acceptor and the hydrogen bond donor are dried separately and then mixed, heated, melted and stirred to form a clear and transparent solvent, and cooled to room temperature for use;
[0015] (2) Preparation of a reverse displacement deposition solution based on a low eutectic solvent: adding a metal salt and a pH buffer to the low eutectic solvent prepared in step (1) and stirring until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0016] (3) Pretreatment of the copper substrate: degreasing, water washing, pickling, water washing and dehydration of the copper substrate in sequence;
[0017] (4) Preparation of metal activation layer by deposition: the copper substrate after dehydration treatment is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) for deposition, the deposition temperature is 35 to 85° C., and the deposition time is 5 to 120 min; then the copper substrate is taken out for washing, and then blow-dried or air-dried.
[0018] Furthermore, the degreasing and defatting solution used for degreasing and defatting in step (3) comprises 25-45 g / l ammonia water, 25-40 g / l Na2CO3, 5-30 g / l NaHCO3, 1-5 g / l hexadecyltrimethylammonium bromide, 25-60 g / l Na2SiO3, and the rest is deionized water. When used, the pH value of the degreasing and defatting solution is adjusted to 6.5-7.5; the degreasing and defatting temperature is 50-75°C, and the degreasing time is 1-5 min;
[0019] The pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C and the time is 10-30s;
[0020] The dehydration treatment is to place the copper substrate in ethanol and perform ultrasonic treatment at 40 to 55 KHz for 5 to 15 minutes.
[0021] Furthermore, when the degreasing and degreasing solution is used, its pH is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5.
[0022] Furthermore, in step (4), compressed air or a hair dryer is used for cold air drying, or the mixture is dried naturally.
[0023] The third aspect of the present invention provides the use of the metal activation layer prepared by the above application in chemical plating catalysis.
[0024] Beneficial effects of the present invention:
[0025] 1. The reverse displacement deposition liquid based on a low eutectic solvent of the present invention causes a potential difference between copper and nickel or cobalt, so that the potential of copper can be lower than that of cobalt or nickel, thereby realizing reverse displacement, thereby preparing a cobalt or nickel metal layer on the copper surface, so as to realize the use of nickel and cobalt metal activation processes to replace palladium activation processes, which has very important practical and theoretical significance; and since the reverse displacement deposition liquid of the present invention adopts a low eutectic solvent system, it will effectively avoid the precipitation and decomposition of metal salts, as well as the side reaction of the reducing agent with water to produce hydrogen, which directly causes defects such as pinholes on the surface of the metal layer, affecting the bonding strength, corrosion resistance and other properties.
[0026] 2. The reverse displacement deposition liquid based on a low eutectic solvent of the present invention is used in the preparation of a metal activation layer by reverse displacement on a copper surface. The obtained pure cobalt metal layer or pure nickel metal layer has a certain catalytic activity for sodium hypophosphite, and its effect is comparable to that of palladium catalysis.
[0027] 3. The reverse displacement deposition liquid based on a low eutectic solvent of the present invention is used in the preparation of a metal activation layer by reverse displacement on a copper surface. Since the use of a low eutectic solvent will not cause a hydrogen evolution side reaction, it can be ensured that the prepared pure cobalt metal layer or pure nickel metal layer has excellent bonding strength, good corrosion resistance and a relatively stable deposition rate, and has good density.
[0028] 4. The reverse displacement deposition solution based on a low eutectic solvent of the present invention is used in the preparation of a metal activation layer by reverse displacement on a copper surface, which is simple to operate and low in cost.
[0029] 5. The reverse displacement deposition liquid based on a low eutectic solvent of the present invention is used in the preparation of a metal activation layer by reverse displacement on a copper surface. No other impurity elements need to be introduced during the deposition process, thus avoiding defects such as black spots that may occur during subsequent operations.
[0030] 6. The reverse displacement deposition liquid based on a low eutectic solvent of the present invention is used in the preparation of a metal activation layer by reverse displacement on a copper surface. Due to the use of a low eutectic solvent, the stability of the working liquid can be ensured, thereby achieving a long service life of the working liquid. DETAILED DESCRIPTION
[0031] The present invention is further explained below in conjunction with the examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0032] The ammonia water mentioned below refers to industrial ammonia water, which is an aqueous solution containing 25% to 28% ammonia.
[0033] The crystal water contained in the following compounds is not included in the mass.
[0034] A reverse displacement deposition solution based on a deep eutectic solvent, comprising a metal salt, a pH buffer and a deep eutectic solvent;
[0035] The metal salt is a nickel salt or a cobalt salt, wherein the nickel salt includes one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite, and the cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate;
[0036] The pH buffer includes tetramethylammonium hydroxide or ammonium bisulfate;
[0037] The low eutectic solvent is prepared by drying a hydrogen bond acceptor and a hydrogen bond donor respectively, mixing them in a molar ratio of 1:1 to 3, heating, melting, and stirring to form a clear and transparent solvent; the hydrogen bond acceptor includes one or more of betaine, choline chloride, and tetramethylammonium chloride; the hydrogen bond donor includes one or more of polyols, carboxylic acids, amino acids, and urea, the polyols include ethylene glycol and pentaerythritol, the carboxylic acids include tartaric acid and citric acid, and the amino acids include glycine;
[0038] The content of the metal salt is 5 to 180 g / l, the content of the pH buffer is 1 to 20 g / l, and the balance is a low eutectic solvent.
[0039] The application of the above-mentioned reverse displacement deposition solution based on a low eutectic solvent in the preparation of a metal activation layer by reverse displacement on a copper surface comprises the following steps:
[0040] (1) Preparation of a low eutectic solvent: The hydrogen bond acceptor and the hydrogen bond donor are dried separately and then mixed, heated, melted and stirred to form a clear and transparent solvent, and cooled to room temperature for use;
[0041] (2) Preparation of a reverse displacement deposition solution based on a low eutectic solvent: adding a metal salt and a pH buffer to the low eutectic solvent prepared in step (1) and stirring until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0042] (3) Pretreatment of the copper substrate: degreasing, water washing, pickling, water washing and dehydration of the copper substrate in sequence;
[0043] The degreasing and degreasing solution used for degreasing and degreasing includes 25-45g / l ammonia water, 25-40g / l Na2CO3, 5-30g / l NaHCO3, 1-5g / l hexadecyltrimethylammonium bromide, 25-60g / l Na2SiO3, and the rest is deionized water. When used, the pH value of the degreasing and degreasing solution is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid. The dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5. The temperature for degreasing and degreasing is 50-75°C, and the time is 1-5min.
[0044] The pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C and the time is 10-30s;
[0045] The dehydration treatment is to place the copper substrate in ethanol and perform ultrasonic treatment at 40 to 55 KHz for 5 to 15 minutes;
[0046] (4) Preparation of metal activation layer by deposition: the copper substrate after dehydration treatment is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) for deposition, the deposition temperature is 35 to 85° C., the deposition time is 5 to 120 min, and then taken out for washing, and then blow-dried or air-dried; the blow-drying is to use compressed air or a hair dryer to blow dry with cold air, and the air-drying is to dry naturally.
[0047] The metal activation layer prepared by the above application is used in chemical plating catalysis.
[0048] The adhesion of the parts in the following embodiments is tested with reference to the cross-hatch test in 2.8 Scribe and Cross-hatch Test in GBT5270-2005 "Review of Test Methods for Adhesion Strength of Electrodeposited and Chemically Deposited Metal Coatings on Metal Substrates"; the corrosion resistance is tested with reference to 5.2.2 Neutral Salt Spray Test (NSS) in GBT10125-2021 "Artificial Atmosphere Corrosion Test Salt Spray Test"; the thickness of the coating is measured with reference to GBT6462-2005 "Microscope Method for Measuring Thickness of Metal and Oxide Coatings"; the density of the coating is measured with reference to QBT3823-1999 "Test Method for Porosity of Metal Coatings on Light Industrial Products"; TEM-EDS-Mapping is used to detect whether the coating is pure cobalt metal element or pure nickel metal element.
[0049] The degreasing and degreasing solution in the following examples consists of 35 g / l ammonia water, 35 g / l Na2CO3, 25 g / l NaHCO3, 3 g / l hexadecyltrimethylammonium bromide, 40 g / l Na2SiO3 and deionized water, and its pH is adjusted to 6.5 using dilute ammonia water (prepared by mixing ammonia water and deionized water in a volume ratio of 1:1) or dilute sulfuric acid (prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:5).
[0050] Example 1
[0051] (1) Preparation of a low eutectic solvent: dried betaine and ethylene glycol are mixed in a molar ratio of 1:2, heated, melted and stirred to form a clear and transparent solvent, and cooled to room temperature for use;
[0052] (2) Preparation of a displacement deposition solution based on a low eutectic solvent: Add nickel sulfate and ammonium bisulfate to the low eutectic solvent prepared in step (1) at a nickel sulfate concentration of 150 g / l and an ammonium bisulfate concentration of 15 g / l, and stir until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0053] (3) Pretreatment of copper substrate: first, place the copper substrate in a degreasing and degreasing solution at 65°C for 3 minutes, then take it out and rinse it with deionized water, then place it in a hydrochloric acid solution at 25°C (the volume ratio of concentrated hydrochloric acid to deionized water is 1:1.5) for pickling for 25 seconds, then take it out and rinse it with deionized water, finally place it in ethanol for ultrasonic dehydration at 55KHz for 10 minutes, then take it out for use;
[0054] (4) Preparation of metal activation layer by deposition: The dehydrated copper substrate is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) at 55° C. for 15 min, then taken out and washed with deionized water, and then blown dry with compressed air.
[0055] Example 2
[0056] (1) Preparation of a low eutectic solvent: Mix dried choline chloride and ethylene glycol in a molar ratio of 1:2.5, heat, melt, and stir to form a clear and transparent solvent, and cool to room temperature for use;
[0057] (2) Preparation of a displacement deposition solution based on a low eutectic solvent: Add nickel sulfate and ammonium bisulfate to the low eutectic solvent prepared in step (1) at a nickel sulfate concentration of 180 g / l and an ammonium bisulfate concentration of 20 g / l and stir until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0058] (3) Pretreatment of copper substrate: first, place the copper substrate in a degreasing and degreasing solution at 65°C for 3 minutes, then take it out and rinse it with deionized water, then place it in a 25°C hydrochloric acid solution ((the volume ratio of concentrated hydrochloric acid and deionized water is 1:2) for pickling for 20 seconds, then take it out and rinse it with deionized water, finally place it in ethanol and perform ultrasonic dehydration treatment at 45KHz for 8 minutes, then take it out for use;
[0059] (4) Preparation of metal activation layer by deposition: The dehydrated copper substrate is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) at 60° C. for 15 min, then taken out and washed with deionized water, and then blown dry with compressed air.
[0060] Example 3
[0061] (1) Preparation of a low eutectic solvent: Mix dried choline chloride and butanediol in a molar ratio of 1:2.5, heat, melt, and stir to form a clear and transparent solvent, and cool to room temperature for use;
[0062] (2) Preparation of a displacement deposition solution based on a low eutectic solvent: adding cobalt sulfate and ammonium bisulfate to the low eutectic solvent prepared in step (1) at a cobalt sulfate concentration of 180 g / l and an ammonium bisulfate concentration of 18 g / l and stirring until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0063] (3) Pretreatment of copper substrate: first, place the copper substrate in a degreasing and degreasing solution at 65°C for 3 minutes, then take it out and rinse it with deionized water, then place it in a hydrochloric acid solution at 25°C (the volume ratio of concentrated hydrochloric acid to deionized water is 1:1.5) for pickling for 25 seconds, then take it out and rinse it with deionized water, finally place it in ethanol for ultrasonic dehydration treatment at 45KHz for 8 minutes, then take it out for use;
[0064] (4) Preparation of metal activation layer by deposition: The dehydrated copper substrate is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) at 60° C. for 45 min, then taken out and washed with deionized water, and then blown dry with compressed air.
[0065] Example 4
[0066] (1) Preparation of a low eutectic solvent: Mix dried choline chloride and ethylene glycol in a molar ratio of 1:3, heat, melt, and stir to form a clear and transparent solvent, and cool to room temperature for use;
[0067] (2) Preparation of a displacement deposition solution based on a low eutectic solvent: adding cobalt sulfate and ammonium bisulfate to the low eutectic solvent prepared in step (1) at a cobalt sulfate concentration of 170 g / l and an ammonium bisulfate concentration of 15 g / l and stirring until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent;
[0068] (3) Pretreatment of copper substrate: first, place the copper substrate in a degreasing and degreasing solution at 65°C for 3 minutes, then take it out and rinse it with deionized water, then place it in a hydrochloric acid solution at 25°C (the volume ratio of concentrated hydrochloric acid to deionized water is 1:2) for 30 seconds, then take it out and rinse it with deionized water, finally place it in ethanol and perform ultrasonic dehydration treatment at 45KHz for 8 minutes, then take it out for use;
[0069] (4) Preparation of metal activation layer by deposition: The dehydrated copper substrate is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) at 60° C. for 45 min, then taken out and washed with deionized water, and then blown dry with compressed air.
[0070] The performance of the products obtained in each embodiment was tested, and the test results are shown in Table 1.
[0071] Table 1
[0072]
[0073]
Claims
1. A reverse displacement deposition solution based on a deep eutectic solvent, characterized in that: including metal salts, pH buffers, and deep eutectic solvents; The metal salt is a nickel salt or a cobalt salt, wherein the nickel salt includes one or more of nickel chloride, nickel sulfamate, nickel acetate, nickel sulfate, and nickel hypophosphite, and the cobalt salt includes one or more of cobalt chloride, cobalt acetate, cobalt sulfate, and cobalt sulfamate; The pH buffer includes tetramethylammonium hydroxide or ammonium bisulfate; The low eutectic solvent is prepared by drying a hydrogen bond acceptor and a hydrogen bond donor respectively, mixing them in a molar ratio of 1:1 to 3, heating, melting, and stirring to form a clear and transparent solvent; the hydrogen bond acceptor includes one or more of betaine, choline chloride, and tetramethylammonium chloride; the hydrogen bond donor includes one or more of polyols, carboxylic acids, amino acids, and urea, the polyols include ethylene glycol and pentaerythritol, the carboxylic acids include tartaric acid and citric acid, and the amino acids include glycine; The content of the metal salt is 5 to 180 g / l, the content of the pH buffer is 1 to 20 g / l, and the balance is a low eutectic solvent.
2. The use of the reverse displacement deposition solution based on a low eutectic solvent according to claim 1 in preparing a metal activation layer by reverse displacement on a copper surface, characterized in that: When applied, the following steps are included: (1) Preparation of a low eutectic solvent: The hydrogen bond acceptor and the hydrogen bond donor are dried separately and then mixed, heated, melted and stirred to form a clear and transparent solvent, and cooled to room temperature for use; (2) Preparation of a reverse displacement deposition solution based on a low eutectic solvent: adding a metal salt and a pH buffer to the low eutectic solvent prepared in step (1) and stirring until the solution becomes clear and transparent to prepare a reverse displacement deposition solution based on a low eutectic solvent; (3) Pretreatment of the copper substrate: degreasing, water washing, pickling, water washing and dehydration of the copper substrate in sequence; (4) Preparation of metal activation layer by deposition: the copper substrate after dehydration treatment is placed in the reverse displacement deposition solution based on the low eutectic solvent prepared in step (2) for deposition, the deposition temperature is 35 to 85° C., and the deposition time is 5 to 120 min; then the copper substrate is taken out for washing, and then blow-dried or air-dried.
3. The use according to claim 2, characterized in that: The degreasing and degreasing solution used for degreasing and degreasing in step (3) comprises 25-45 g / l ammonia water, 25-40 g / l Na2CO3, 5-30 g / l NaHCO3, 1-5 g / l hexadecyltrimethylammonium bromide, 25-60 g / l Na2SiO3, and the rest is deionized water. When used, the pH value of the degreasing and degreasing solution is adjusted to 6.5-7.5; the degreasing and degreasing temperature is 50-75°C, and the degreasing time is 1-5 min; The pickling solution used for pickling is a hydrochloric acid solution with a volume ratio of concentrated hydrochloric acid to deionized water of 1:1-3 or a sulfuric acid solution with a volume ratio of concentrated sulfuric acid to deionized water of 1:1-3; the pickling temperature is 20-35°C and the time is 10-30s; The dehydration treatment is to place the copper substrate in ethanol and perform ultrasonic treatment at 40 to 55 KHz for 5 to 15 minutes.
4. The use according to claim 3, characterized in that: When the degreasing and degreasing solution is used, its pH is adjusted to 6.5-7.5 with dilute ammonia water or dilute sulfuric acid; the dilute ammonia water is prepared by mixing ammonia water and deionized water in a volume ratio of 1:1, and the dilute sulfuric acid is prepared by mixing concentrated sulfuric acid and deionized water in a volume ratio of 1:
5.
5. The use according to claim 2, characterized in that: In step (4), use compressed air or a hair dryer to blow dry with cold air, or dry naturally.
6. Use of the metal activation layer prepared by the use according to any one of claims 2 to 5 in chemical plating catalysis.
Citation Information
Cited By
Chemical tin plating solution based on eutectic solvent and applied to PCB copper foil and application of chemical tin plating solution
CN120249952A