Nickel-based solid oxide fuel cell anode catalyst material as well as preparation method and application thereof
Through the preparation of the anode catalyst material of nickel-based solid oxide fuel cell, the problem of low electrolytic performance of anode materials at high temperatures is solved, and effective catalytic and electrolytic performance improvement of hydrocarbon fuels such as methane is achieved.
Patent Information
- Application Number
- CN202411021139.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Existing solid oxide fuel cell anode materials are prone to lattice defects at high temperatures, resulting in loss of oxygen vacancies and oxygen channels, making it difficult to meet the requirements of reverse operation electrolytic mode for oxygen ion conductivity and catalytic performance, especially when methane is introduced. The electrolytic performance is low when used in the same hydrocarbon fuel.
The chemical structure of the anode catalyst material of the nickel-based solid oxide fuel cell is Ni/Ce0.8Zr0.2O2. The high temperature stability of the material is improved by specific preparation methods, such as the components mixing, drying and calcining process in steps S1-S4. and oxygen ion conduction capacity enhance the performance of catalytic methane oxidation.
The catalytic oxidation performance and oxygen ion conduction capability of the anode of solid oxide fuel cell is improved, the electrolytic voltage in the reverse running electrolytic mode is reduced, and the processing capacity of hydrocarbon fuels such as methane is enhanced.
Smart Images

Figure CN118957638A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of solid oxide battery technology, and in particular to nickel-based solid oxide fuel cell anode catalyst materials, preparation methods and applications. Background Art
[0002] In addition to conventional water electrolysis to produce hydrogen, solid oxide fuel cell reverse electrolysis mode (SOEC) can also electrolyze water to produce hydrogen at high temperature. Solid oxide fuel cell water electrolysis has the advantages of low overpotential and low power consumption, and has higher electrolysis efficiency. In the process of solid oxide fuel cell water electrolysis, anode oxidation consumes more electricity. Studies have found that supplying hydrocarbon fuels such as methane in the form of chemical energy can provide part of the energy required for water electrolysis and reduce power input.
[0003] However, methane (CH 4 ) is a structurally stable hydrocarbon with high bond energy and difficult activation; therefore, noble metal catalysts and metal oxide catalysts such as nickel can be used in the anode of solid oxide fuel cells to catalyze the oxidation of methane to reduce the anode overpotential; however, in addition to using catalysts to catalyze the oxidation of methane (CH 4 ) for catalytic oxidation, SOEC also requires the anode material to exhibit good O 2- conductivity to ensure that the cathode O 2- Transfer to the oxidative active sites in the anode. In common oxygen ion conductors, CeO 2 The base material has high oxygen storage capacity and oxygen ion conductivity. However, CeO 2 The base material is prone to lattice defects at high temperatures, resulting in the loss of oxygen vacancies and oxygen channels. Therefore, the current solid oxide fuel cell anode materials have low electrolysis performance and are difficult to meet the requirements of the reverse electrolysis mode of the solid oxide fuel cell when hydrocarbon fuels such as methane are introduced. Summary of the invention
[0004] In view of this, the present application provides a nickel-based solid oxide fuel cell anode catalyst material and a preparation method and application thereof, which are used to solve the technical problem in the prior art that the electrolysis performance of the solid oxide fuel cell anode material is low when hydrocarbon fuels such as methane are introduced.
[0005] The first aspect of the present application provides a nickel-based solid oxide fuel cell anode catalyst material, the chemical structure of which is: Ni / Ce 0.8 Zr 0.2 O 2 .
[0006] Preferably, in the nickel-based solid oxide fuel cell anode catalyst material, the doping amount of Ni is 5 wt %.
[0007] The second aspect of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, which is the first method for preparing the nickel-based solid oxide fuel cell anode catalyst material described in the first aspect. The preparation method comprises the steps of:
[0008] Step S1, adding cerium salt and zirconium salt into deionized water and stirring to obtain Ce 0.8 Zr 0.2 O 2 Carrier solution;
[0009] Step S2: Add nickel salt to Ce 0.8 Zr 0.2 O 2 Stir evenly in the carrier solution to obtain Ni / Ce 0.8 Zr 0.2 O solution;
[0010] Step S3: adding ammonium carbonate solution to Ni / Ce 0.8 Zr 0.2 O solution and heated and stirred until dehydration to obtain Ni / Ce 0.8 Zr 0.2 O solid gel;
[0011] Step S4: Ni / Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
[0012] Preferably, in step S2, the Ce 0.8 Zr 0.2 O 2 Ce in carrier solution 0.8 Zr 0.2 O 2 The mass ratio of the nickel to the nickel salt is 1:0.02-0.1.
[0013] Preferably, in step S1, the cerium salt is selected from Ce(NO 3 ) 3 6H 2 O, zirconium salt is selected from Zr(NO 3 ) 4 ·5H 2 O;
[0014] In step S2, the nickel salt is selected from Ni(NO 3 ) 2 6H 2 O.
[0015] Preferably, in step S1, the stirring temperature is 70 to 90° C. and the stirring time is 2 to 6 hours;
[0016] In step S3, the temperature of heating and stirring is 70-100°C;
[0017] In step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
[0018] Preferably, in step S1, the Ce(NO 3 ) 3 6H 2 O was added in an amount of 6 g, and the Zr(NO 3 ) 4 ·5H 2 The amount of O added was 1.4831 g;
[0019] In step S3, the concentration of the ammonium carbonate solution is 1-3 mol / L, and the amount added is 80-120 mL.
[0020] The third aspect of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, which is the second method for preparing the nickel-based solid oxide fuel cell anode catalyst material described in the first aspect. The preparation method comprises the steps of:
[0021] Step S1, dissolving cerium salt and zirconium salt in deionized water, adding ammonium carbonate solution and heating and stirring until dehydration, to obtain Ce 0.8 Zr 0.2 O solid gel;
[0022] Step S2: Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ce 0.8 Zr 0.2 O carrier material;
[0023] Step S3: Ce 0.8 Zr 0.2 O carrier material is added to the nickel salt solution for impregnation to obtain Ni / Ce 0.8 Zr 0.2 O precursor;
[0024] Step S4: Ni / Ce 0.8 Zr 0.2 O precursor is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
[0025] Preferably, in step S3, the Ce 0.8Zr 0.2 Ce in O support material 0.8 Zr 0.2 O 2 The mass ratio of the nickel to the nickel salt solution is 1:0.02-0.1.
[0026] Preferably, in step S1, the cerium salt is selected from Ce(NO 3 ) 3 6H 2 O, zirconium salt is selected from Zr(NO 3 ) 4 ·5H 2 O, in step S3, the nickel salt is selected from Ni(NO 3 ) 2 6H 2 O.
[0027] Preferably, in step S1, the temperature of heating and stirring is 70-100°C;
[0028] In step S2 and step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
[0029] Preferably, in step S1, the Ce(NO 3 ) 3 6H 2 O was added in an amount of 6 g, and the Zr(NO 3 ) 4 ·5H 2 The amount of O added is 1.4831 g, the concentration of the ammonium carbonate solution is 1-3 mol / L, and the amount added is 80-120 mL.
[0030] The fourth aspect of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, which is the third method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to the first aspect. The preparation method comprises the following steps:
[0031] Step S1, adding cerium salt and zirconium salt into deionized water and stirring to obtain Ce 0.8 Zr 0.2 O 2 Carrier solution;
[0032] Step S2: Add nickel salt to Ce 0.8 Zr 0.2 O 2 Stir evenly in the carrier solution to obtain Ni / Ce 0.8 Zr 0.2 O solution;
[0033] Step S3: Add citric acid to Ni / Ce 0.8 Zr 0.2 O solution and heated and stirred until dehydration to obtain Ni / Ce 0.8 Zr 0.2 O solid gel;
[0034] Step S4: Ni / Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
[0035] Preferably, in step S3, the Ce 0.8 Zr 0.2 O 2 Ce in carrier solution 0.8 Zr 0.2 O 2 The mass ratio of the nickel to the nickel salt is 1:0.02-0.1.
[0036] Preferably, in step S1, the cerium salt is selected from Ce(NO 3 ) 3 6H 2 O, zirconium salt is selected from Zr(NO 3 ) 4 ·5H 2 O.
[0037] In step S2, the nickel salt is selected from Ni(NO 3 ) 2 6H 2 O.
[0038] Preferably, in step S3, the temperature of heating and stirring is 70-100° C.;
[0039] In step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
[0040] Preferably, in step S1, the Ce(NO 3 ) 3 6H 2 O was added in an amount of 6 g, and the Zr(NO 3 ) 4 ·5H 2 The amount of O added is 1.4831 g. In step S3, the citric acid and the Ce 0.8 Zr 0.2 O 2 The molar ratio of the total molar number of metal ions in the carrier solution is 1.5-2.5:1.
[0041] The fifth aspect of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, which is the fourth method for preparing a nickel-based solid oxide fuel cell anode catalyst material described in the first aspect. The preparation method comprises the steps of:
[0042] Step S1, dissolving cerium salt and zirconium salt in deionized water, adding citric acid and heating and stirring until dehydration, to obtain Ce 0.8 Zr 0.2 O solid gel;
[0043] Step S2: Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ce 0.8 Zr 0.2 O carrier material;
[0044] Step S3: Ce 0.8 Zr 0.2 O carrier material is added to the nickel salt impregnation solution for impregnation to obtain Ni / Ce 0.8 Zr 0.2 O precursor;
[0045] Step S4: Ni / Ce 0.8 Zr 0.2 O precursor is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
[0046] Preferably, in step S3, the Ce 0.8 Zr 0.2 Ce in O support material 0.8 Zr 0.2 O 2 The mass ratio of the nickel to the nickel salt solution is 1:0.02-0.1.
[0047] Preferably, in step S1, the cerium salt is selected from Ce(NO 3 ) 3 6H 2 O, zirconium salt is selected from Zr(NO 3 ) 4 ·5H 2 O;
[0048] In step S2, the nickel salt is selected from Ni(NO 3 ) 2 6H 2 O.
[0049] Preferably, in step S1, the temperature of the heating and stirring is 70-100°C.
[0050] In step S2 and step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
[0051] Preferably, in step S1, the Ce(NO 3 ) 3 6H 2 O was added in an amount of 6 g, and the Zr(NO 3 ) 4 ·5H 2 The amount of O added was 1.4831 g, citric acid and the Ce 0.8 Zr 0.2 O 2 The molar ratio of the total molar number of metal ions in the carrier solution is 1.5-2.5:1.
[0052] The sixth aspect of the present application provides the use of the nickel-based solid oxide fuel cell anode catalyst material described in the first aspect in the preparation of a solid oxide fuel cell.
[0053] Preferably, the application specifically comprises: printing an anode slurry containing the high-temperature solid oxide fuel cell anode catalyst material prepared by the preparation method described in the first aspect onto the anode side of the solid oxide fuel cell, and calcining at high temperature to obtain the anode of the solid oxide fuel cell;
[0054] The high temperature calcination is carried out at a temperature of 850-1200° C. and for a time of 3 hours.
[0055] In summary, the present application provides a nickel-based solid oxide fuel cell anode catalyst material and a preparation method and application thereof. The nickel-based solid oxide fuel cell anode catalyst material provided by the present application uses active metal nickel as a catalyst for the catalytic oxidation of methane, CeO 2 As an oxygen ion conductor, CeO 2 On the one hand, under anoxic or reducing conditions, the surface Ce 4 + Reducing to Ce 3+ , and generate oxygen vacancies, thereby improving its high temperature stability, and Zr doping can also increase the content of oxygen vacancies, thereby improving CeO 2 The high-temperature stability of the crystal structure makes the nickel-based high-temperature solid oxide fuel cell anode material provided in the present application have good catalytic oxidation performance and oxygen ion conductivity, which can reduce the SOEC electrolysis voltage when the solid oxide fuel cell operates in the reverse electrolysis mode, thereby solving the technical problem of low electrolysis performance of the solid oxide fuel cell anode material when hydrocarbon fuels such as methane are introduced in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0057] Figure 1 A scanning electron microscope image of a nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 of the present application;
[0058] Figure 2 IV curve results of the battery prepared by the nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 of the present application in argon and methane atmospheres;
[0059] Figure 3 Impedance spectra of batteries prepared from the nickel-based high-temperature solid oxide fuel cell anode catalyst materials provided in Examples 1-4 of the present application in argon, methane and air atmospheres;
[0060] Figure 4 The constant-pressure electrolysis performance graphs of the battery prepared from the nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 of the present application in air, argon and methane atmospheres, FIG a is a constant-pressure electrolysis performance graph in air atmosphere, FIG b is a constant-pressure electrolysis performance graph in air atmosphere, and FIG c is a constant-pressure electrolysis performance graph in air atmosphere;
[0061] Figure 5 for Figure 2 Black and white comparison chart;
[0062] Figure 6 for Figure 3 Black and white comparison chart;
[0063] Figure 7 for Figure 4 Black and white comparison chart. DETAILED DESCRIPTION
[0064] The present application provides a nickel-based solid oxide fuel cell anode catalyst material and a preparation method and application thereof, which are used to solve the technical problem in the prior art that the electrolysis performance of the solid oxide fuel cell anode material is low when hydrocarbon fuels such as methane are introduced.
[0065] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0066] Example 1
[0067] Example 1 of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material. The preparation method comprises: 0.8 Zr 0.2 O 2 Steps for carrier solution, configuration of Ni / Ce 0.8 Zr 0.2 O solution steps, preparation of Ni / Ce 0.8 Zr 0.2 O gel step and calcination step.
[0068] Among them, configure Ce 0.8 Zr 0.2 O 2 The steps of the carrier solution include: at room temperature, 6 g of Ce(NO 3 ) 3 6H 2 O, 1.4831 g of Zr(NO 3 ) 4 ·5H 2 O were dissolved in 50 mL of deionized water and stirred vigorously for 4 h to obtain Ce 0.8 Zr 0.2 O 2 Carrier solution.
[0069] Configuration Ni / Ce 0.8 Zr 0.2 O solution steps include: 0.8 Zr 0.2 O 2 Ni(NO 3 ) 2 6H 2 O is stirred evenly to obtain Ni / Ce 0.8 Zr 0.2 O 2 Solution.
[0070] Preparation of Ni / Ce 0.8 Zr 0.2 The steps of O gel include: 0.8 Zr 0.2 O 2The molar ratio of the total number of metal ions and citric acid is 1:2. 0.8 Zr 0.2 O 2 Add citric acid twice the molar number of metal ions into the solution and slowly evaporate it by stirring at 90°C until the solution is dehydrated to a dry gel state to obtain Ni / Ce 0.8 Zr 0.2 O 2 gel.
[0071] The calcination step includes: drying at 100°C for 12 hours, calcining the obtained solid at 500°C for 5 hours at a heating rate of 3°C / min in an air atmosphere to obtain a nickel-based high-temperature solid oxide fuel cell anode catalyst material, marked as 5% Ni / Ce 0.8 Zr 0.2 O 2 -SG, its electron microscope image is as follows Figure 1 As shown in Figure a.
[0072] Example 2
[0073] Example 2 of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, the preparation method comprising preparing Ce 0.8 Zr 0.2 O gel steps, preparation of Ce 0.8 Zr 0.2 O support step, impregnation step and preparation of Ni / Ce 0.8 Zr 0.2 Steps of O.
[0074] Among them, preparation of Ce 0.8 Zr 0.2 The steps of O gelling include: mixing 6 g of Ce(NO 3 ) 3 6H 2 O, 1.4831 g of Zr(NO 3 ) 4 ·5H 2 O were dissolved in 100 mL of deionized water and citric acid was added at a molar amount of 2 times that of the metal ions, and stirred to evaporate slowly until the solution was dehydrated to a dry gel state to obtain Ce 0.8 Zr 0.2 O gel.
[0075] Preparation of Ce 0.8 Zr 0.2 The steps of O carrier include: 0.8 Zr 0.2After the O gel was dried at 100 °C for 12 h, the obtained solid was calcined at 500 °C for 5 h in an air atmosphere at a heating rate of 3 °C / min to obtain Ce 0.8 Zr 0.2 O carrier.
[0076] The impregnation steps include: 0.8 Zr 0.2 O carrier and Ni in a mass ratio of 1:0.05. First, Ni(NO 3 ) 2 6H 2 O was dissolved in 20 mL of deionized water, and then 1 g of Ce was added 0.8 Zr 0.2 O carrier was impregnated for 3 h to obtain Ce loaded with Ni component. 0.8 Zr 0.2 O carrier.
[0077] Preparation of Ni / Ce 0.8 Zr 0.2 The step of O comprises: drying at 100°C for 12 hours, 0.8 Zr 0.2 The O support was calcined at 500 °C for 5 h in an air atmosphere at a heating rate of 3 °C / min to obtain a nickel-based high-temperature solid oxide fuel cell anode catalyst material, labeled as 5% Ni / Ce 0.8 Zr 0.2 O 2 -SG-Im, its electron microscope image is as follows Figure 1 As shown in Figure b.
[0078] Example 3
[0079] Example 3 of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material. The preparation method comprises: 0.8 Zr 0.2 O 2 Steps for carrier solution, configuration of Ni / Ce 0.8 Zr 0.2 O solution steps, preparation of Ni / Ce 0.8 Zr 0.2 O gel step and calcination step.
[0080] Among them, configure Ce 0.8 Zr 0.2 O 2 The steps of the carrier solution include: at 80°C, 6 g of Ce(NO 3 ) 3 6H 2 O, 1.4831 g of Zr(NO3 ) 4 ·5H 2 O were dissolved in 50 mL of deionized water and stirred vigorously for 4 h to obtain Ce 0.8 Zr 0.2 O 2 Carrier solution.
[0081] Configuration Ni / Ce 0.8 Zr 0.2 O solution steps include: 0.8 Zr 0.2 O 2 Ni(NO 3 ) 2 6H 2 O is stirred evenly to obtain Ni / Ce 0.8 Zr 0.2 O 2 Solution.
[0082] Preparation of Ni / Ce 0.8 Zr 0.2 The steps of O gelling include: adding 100 mL (NH 4 ) 2 CO 3 solution (2 mol / L) and slowly evaporated by stirring at 80°C until the solution was dehydrated to a dry gel state to obtain Ni / Ce 0.8 Zr 0.2 O 2 gel.
[0083] The calcination step includes: drying at 100°C for 12 hours, calcining the obtained solid at 500°C for 5 hours at a heating rate of 3°C / min in an air atmosphere to obtain a nickel-based high-temperature solid oxide fuel cell anode catalyst material, marked as 5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy, its electron microscope image is as follows Figure 1 As shown in Figure c.
[0084] Example 4
[0085] Example 4 of the present application provides a method for preparing a nickel-based high-temperature solid oxide fuel cell anode catalyst material, the preparation method comprising preparing Ce 0.8 Zr 0.2 O gel steps, preparation of Ce 0.8 Zr 0.2 O support step, impregnation step and preparation of Ni / Ce 0.8 Zr 0.2 Steps of O.
[0086] Among them, preparation of Ce 0.8 Zr 0.2 The steps of O gelling include: mixing 6 g of Ce(NO 3 ) 3 6H 2 O, 1.4831 g of Zr(NO 3 ) 4 ·5H 2 O were dissolved in 50 mL of deionized water and 100 mL of (NH 4 ) 2 CO 3 The solution (2 mol / L) was stirred and slowly evaporated until the solution was dehydrated to a dry gel state to obtain Ce 0.8 Zr 0.2 O gel.
[0087] Preparation of Ce 0.8 Zr 0.2 The step of O carrier comprises: drying at 100°C for 12 hours, 0.8 Zr 0.2 The O gel was calcined at 500 °C for 5 h in air at a heating rate of 3 °C / min to obtain Ce 0.8 Zr 0.2 O carrier.
[0088] The impregnation steps include: 0.8 Zr 0.2 O carrier and Ni in a mass ratio of 1:0.05. First, Ni(NO 3 ) 2 6H 2 O was dissolved in 20 mL of deionized water, and then 1 g of Ce was added 0.8 Zr 0.2 O carrier was impregnated for 3 h to obtain Ce loaded with Ni component. 0.8 Zr 0.2 O carrier.
[0089] Preparation of Ni / Ce 0.8 Zr 0.2 The step of O comprises: drying at 100°C for 12 hours, 0.8 Zr 0.2 The O support was calcined at 500 °C for 5 h in an air atmosphere at a heating rate of 3 °C / min to obtain a nickel-based high-temperature solid oxide fuel cell anode catalyst material, labeled as 5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy-Im, its electron microscope image is as follows Figure 1 As shown in Figure d.
[0090] Experimental Example 1
[0091] The present application conducts performance tests on the nickel-based high-temperature solid oxide fuel cell anode catalyst materials provided in Examples 1-4 to compare the performance differences of the nickel-based high-temperature solid oxide fuel cell anode catalyst materials prepared by different preparation methods.
[0092] The performance test requires the preparation of a solid oxide fuel cell. The assembly process of the solid oxide fuel cell is as follows: using a conventional 8YSZ electrolyte and a Ni-8YSZ cathode as a substrate, using the nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 as an anode material, and using a silver mesh for current collection; the process is to mix the nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 with silver powder in a mass ratio of 1:1, prepare a slurry with 5wt% starch and KS1 adhesive, print the slurry on the anode side of the 8YSZ electrolyte by screen printing, and then calcine at 850 for 3h to prepare a SOEC anode, and the effective area of the anode side is 1.5cm 2 .
[0093] The performance test process includes: placing 4 batteries prepared from the nickel-based high-temperature solid oxide fuel cell anode catalyst material provided in Examples 1-4 in a tubular furnace, purging the anode and cathode with 50 mL / min of argon, heating to 850°C, and maintaining a constant temperature.
[0094] Switch the Ar gas on the anode and cathode sides to H 2 , and H 2 The flow rate of was also 50 mL / min. The catalyst on the anode side and the catalyst on the cathode side were reduced for 1 hour. After reduction, the anode atmosphere was switched to 85 mL / min of Ar gas and purged for 30 minutes. At the same time, the H 2 The flow rate was adjusted to 85 mL / min. After the anode was purged for 30 minutes, 50 mL / min of water vapor was introduced to the cathode side. After stabilization, methane gas was switched and tested using an electrochemical workstation. The tests included IV curves, constant voltage electrolysis, and electrochemical impedance spectroscopy (EIS). Constant voltage electrolysis was tested from 0.2 V to 1.6 V with a gradient of 0.2 V. EIS was tested at different open circuit voltages with a frequency range of 10 6 HZ~10 -2 HZ, amplitude is 30mV.
[0095] Among them, the nickel-based high-temperature solid oxide fuel cell anode catalyst material (5% Ni / Ce 0.8 Zr 0.2 O 2-SG) prepared battery in different atmospheres, IV curve results, electrochemical impedance spectroscopy Figure 2-3 As shown in Figure a, constant voltage electrolysis Figure 4 shown; from Figure 2 The IV curves of the battery in argon atmosphere and methane atmosphere shown in Figure a show that the curves of the two are almost the same, indicating that methane may play a role in reducing the oxygen partial pressure, and it is difficult to catalyze methane oxidation to play a role in reducing the electrolysis voltage of SOEC. Figure 3 The electrochemical impedance spectrum shown in Figure a also shows that the curves of the two are similar. Figure 4 The constant-voltage electrolysis tests shown in Figures bc also show that the constant-voltage electrolysis currents in argon atmosphere and methane atmosphere are similar.
[0096] The nickel-based high-temperature solid oxide fuel cell anode catalyst material (5% Ni / Ce 0.8 Zr 0.2 O 2 -SG-Im) prepared battery IV curve results in different atmospheres, electrochemical impedance spectrum Figure 2-3 As shown in Figure b, constant voltage electrolysis Figure 4 shown; from Figure 2 The IV curves of the battery in argon atmosphere and methane atmosphere shown in Figure b show that the electrolysis voltage of the battery in methane atmosphere is significantly lower. For example, in argon atmosphere, the battery has a lower voltage at 250mA / cm 2 This may be due to the concentration polarization of oxygen precipitated in the pores of the battery anode material, which leads to an increase in the electrolysis voltage. The electrolysis voltage can be significantly reduced in a methane atmosphere because of the catalytic methane oxidation. Figure 3 As can be seen from Figure b, compared with argon atmosphere, within a certain range, the ohmic resistance and polarization resistance of the battery's anode in methane atmosphere are obviously lower, which also shows that the catalytic methane oxidation reaction of the battery's anode is easy, and methane oxidation consumes oxygen at the cathode, thereby significantly reducing the electrolysis voltage, which makes it possible to obtain a higher current during constant voltage electrolysis. As shown in Figure 4, when constant voltage electrolysis is carried out in a methane atmosphere, 5% Ni / Ce 0.8 Zr 0.2 O 2 -SG-Im prepared battery has higher current.
[0097] Among them, the nickel-based high-temperature solid oxide fuel cell anode catalyst material (5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy) prepared battery IV curve results in different atmospheres, electrochemical impedance spectroscopy Figure 2-3 As shown in Figure c, constant voltage electrolysis Figure 4 shown; from Figure 2 The IV curves of the battery in argon atmosphere and methane atmosphere shown in Figure c show that in methane atmosphere, the IV curve of the battery is slightly lower, and the catalytic methane oxidation in the battery anode has only a general effect on reducing the electrolysis voltage, which is slightly better than (5% Ni / Ce 0.8 Zr 0.2 O 2 -SG) to prepare a battery, and Figure 3 As can be seen from Figure c, within a certain range, the ohmic impedance and polarization impedance in the argon atmosphere are lower than those in the methane atmosphere, and the promoting effect of the reduction of oxygen partial pressure is weakened. This may be due to the nickel-based high-temperature solid oxide fuel cell anode catalyst material (5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy) catalytic methane oxidation effect is common reason; such as Figure 4 As shown, when constant voltage electrolysis is carried out in a methane atmosphere, 5% Ni / Ce 0.8 Zr 0.2 O 2 The current of the battery prepared by -Hy is slightly higher.
[0098] The nickel-based high-temperature solid oxide fuel cell anode catalyst material (5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy-Im) prepared battery IV curve results in different atmospheres, electrochemical impedance spectrum Figure 2-3 As shown in Figure d, constant voltage electrolysis Figure 4 shown; from Figure 2 The IV curves of the battery in argon atmosphere and methane atmosphere shown in Figure d show that compared with the argon atmosphere, the 5% Ni / Ce 0.8 Zr 0.2 O 2 The catalytic oxidation activity of the battery anode prepared by -Hy-Im can greatly promote the reduction of the electrolysis voltage. Figure 3 It can be seen from Figure d that within a certain range, the ohmic impedance and polarization impedance in argon atmosphere are lower than those in methane atmosphere, that is, the anode surface is more inclined to oxygen evolution process, and oxygen evolution may occur first on the anode surface of the battery, and then methane oxidation reaction occurs; Figure 4 As shown, when constant voltage electrolysis is carried out in a methane atmosphere, 5% Ni / Ce 0.8 Zr 0.2 O 2 -Hy prepared batteries have higher current.
[0099] Further from Figure 4 It can be seen that 5% Ni / Ce 0.8 Zr 0.2 O2 -Hy-Im, 5% Ni / Ce 0.8 Zr 0.2 O 2 -SG has a better effect on promoting methane oxidation than the other two anode catalyst materials and is suitable as an anode catalyst material to promote SOEC electrolysis when methane and other gases are introduced.
[0100] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A nickel-based solid oxide fuel cell anode catalyst material, characterized in that: The chemical structure is: Ni / Ce 0.8 Zr 0.2 O2.
2. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 1, characterized in that: Includes steps: Step S1, adding cerium salt and zirconium salt into deionized water and stirring to obtain Ce 0.8 Zr 0.2 O2 carrier solution; Step S2: Add nickel salt to Ce 0.8 Zr 0.2 O2 carrier solution was stirred evenly to obtain Ni / Ce 0.8 Zr 0.2 O solution; Step S3: adding ammonium carbonate solution or citric acid to the Ni / Ce 0.8 Zr 0.2 O solution and heated and stirred until dehydration to obtain Ni / Ce 0.8 Zr 0.2 O solid gel; Step S4: Ni / Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
3. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 2, characterized in that: In step S2, the Ce 0.8 Zr 0.2 Ce in O2 carrier solution 0.8 Zr 0.2 The mass ratio of O2 to Ni in the nickel salt is 1:0.02-0.
1.
4. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 2, characterized in that: In step S1, the cerium salt is selected from Ce(NO3)3·6H2O, and the zirconium salt is selected from Zr(NO3)4·5H2O; In step S2, the nickel salt is selected from Ni(NO3)2·6H2O.
5. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 2, characterized in that: In step S3, the temperature of heating and stirring is 70-100°C; In step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
6. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 1, characterized in that: Includes steps: Step S1, dissolving cerium salt and zirconium salt in deionized water, adding ammonium carbonate solution or citric acid, and heating and stirring until dehydration, to obtain Ce 0.8 Zr 0.2 O solid gel; Step S2: Ce 0.8 Zr 0.2 O solid gel is dried and calcined in sequence to obtain Ce 0.8 Zr 0.2 O carrier material; Step S3: Ce 0.8 Zr 0.2 O carrier material is added to the nickel salt solution for impregnation to obtain Ni / Ce 0.8 Zr 0.2 O precursor; Step S4: Ni / Ce 0.8 Zr 0.2 O precursor is dried and calcined in sequence to obtain Ni / Ce 0.8 Zr 0.2 O anode catalyst material.
7. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 6, characterized in that: In step S3, in step S3, the Ce 0.8 Zr 0.2 Ce in O support material 0.8 Zr 0.2 The mass ratio of O2 to Ni in the nickel salt solution is 1:0.02-0.
1.
8. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 6, characterized in that: In step S1, the cerium salt is selected from Ce(NO3)3·6H2O, and the zirconium salt is selected from Zr(NO3)4·5H2O; In step S3, the nickel salt is selected from Ni(NO3)2·6H2O.
9. The method for preparing a nickel-based solid oxide fuel cell anode catalyst material according to claim 6, characterized in that: In step S1, the temperature of heating and stirring is 70-100°C; In step S2 and step S4, the drying temperature is 80-120° C., the time is 8-16 hours, and the calcination temperature is 400-600° C., the time is 4-6 hours.
10. Use of the nickel-based solid oxide fuel cell anode catalyst material according to claim 1 in the preparation of a solid oxide fuel cell.