Titanium oxide loaded oxide catalyst with heterogeneous structure as well as preparation method and application of titanium oxide loaded oxide catalyst

The preparation of heterophase structure titanium oxide supported oxide catalysts was solved by sol-gel method, and the stability and conductivity of PEM electrolytic OER catalysts under high potential conditions were improved, the activity of the catalyst and iridium/ruthenium utilization rate were improved, and the Efficient OER performance improvement.

CN118957641APending Publication Date: 2024-11-15SHENZHEN SENERGY FUEL CELL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411043819.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing PEM electrolytic OER catalyst has poor stability under high potential conditions, and is prone to form a TiO2 layer with poor conductivity, which reduces the catalyst performance and has low iridium utilization.

Method used

The two-phase heterostructure titanium oxide is prepared as the core by sol-gel method, and the heterostructure titanium oxide with high conductivity and large specific surface area is formed by doping the first metal heteroatom and heat treatment, and the second metal oxide particles are loaded. For example, Ir or Ru, a low iridium/ruthenium core-shell catalyst is formed.

Benefits of technology

The activity, durability, and utilization rate of iridium/ruthenium of the PEM electrolytic anode are improved, and the conductivity and surface area of ​​the catalyst are improved, which significantly improves the OER performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a titanium oxide loaded oxide catalyst with a heterogeneous structure as well as a preparation method and application thereof, and belongs to the technical field of fuel cells. The preparation method of the heterogeneous structure titanium oxide loaded oxide catalyst comprises the following steps: S01, hydrolyzing a titanium-containing organic compound precursor in alcohol to prepare a first metal atom doped titanium oxide sol; s02, drying the titanium oxide sol prepared in the step S01 to obtain titanium oxide gel; s03, performing heat treatment on the titanium oxide gel in the step S02 to prepare first metal doped titanium oxide with a two-phase heterostructure; s04, loading second metal oxide particles on the surface of the first metal doped titanium oxide; the heterogeneous structure titanium oxide loaded oxide catalyst is obtained; wherein the second metal is at least one of Ir or Ru. The high-activity and high-durability low-iridium / ruthenium core-shell catalyst is prepared, the utilization rate of iridium / ruthenium is increased, and the dosage of iridium / ruthenium of a PEM electrolyzed water anode is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a titanium oxide-loaded oxide catalyst with a heterogeneous structure, and a preparation method and application thereof. Background Art

[0002] The decarbonization of the global energy sector requires the rapid growth of green hydrogen energy, and electrocatalytic water splitting is considered to be the best method for large-scale hydrogen production. The two mainstream water splitting technologies currently used for hydrogen production are proton exchange membrane water electrolyzers (PEMWEs) and alkaline water electrolyzers. Compared with alkaline electrolysis, PEMWEs have the advantages of higher energy efficiency, higher current density and purer hydrogen products, faster response speed, etc., which are very suitable for combination with intermittent energy sources (such as wind and solar energy) to provide electrolytic hydrogen for long-term energy storage or mobility of fuel cells. At present, the large-scale application of PEM electrolyzers is still hindered by their high capital costs. In a strongly acidic working environment, commercial PEMWEs require the use of precious metal catalysts. For example, platinum is usually used for the hydrogen evolution reaction (HER) at the cathode, while iridium is used for the oxygen evolution reaction (OER) at the anode. Among them, OER involves four electron transfer steps, and its energy barrier is much higher than HER. Usually, 5 times the amount of iridium is used at the anode than the cathode platinum to achieve optimal performance. This reliance on iridium-based catalysts has hindered the widespread adoption of this technology. Therefore, a major focus in advancing PEMWE technology is to develop OER electrocatalysts with low iridium loading, high activity, high durability, and acid resistance.

[0003] At present, low-iridium catalysts are mainly concentrated in two types: doped and supported. These two types of low-iridium catalysts show higher catalytic activity than iridium oxides, such as Sn, Ta, Mo, Gd, Ce, etc. doped IrO2, IrNiO X Core-shell structure, IrO X / ATO, etc. However, doped iridium oxide catalysts have the problem of unstable crystal phase. Metal elements are easily dissolved and the structure collapses under electrolysis conditions, resulting in performance degradation. Loading iridium oxide on a carrier is an effective way to improve its dispersion and reduce its dosage. It can not only effectively improve the utilization rate of Ir through the carrier, but also regulate the electronic structure of the active center through the interaction between the precious metal and the carrier, thereby improving the intrinsic activity of the precious metal. However, since OER reacts at high potential, the catalyst carrier has high requirements for anti-oxidation, anti-corrosion and high conductivity. Currently common ones are SnO2, TiO2, SiO2, TiO2, NiO x TiO2 has high resistance to anodic corrosion and is one of the ideal carriers. It is also currently used in commercial OER catalysts. However, TiO2 has a small specific surface area and poor conductivity, which leads to low Ir utilization and reduced OER activity. In order to improve conductivity, a common method is to prepare a non-stoichiometric metastable phase Tin O 2n-7 However, under the high potential environment of the water electrolysis anode, a TiO2 layer with poor conductivity will be formed, reducing the OER performance.

[0004] In order to overcome the limitations of poor conductivity and small specific surface area, doping can be used to improve the conductivity of TiO2. Doping with transition metals such as Nb and W can improve the conductivity through the dd energy band interaction between the two. Heteroatom doping can also increase the oxygen vacancies of TiO2. At the same time, heterostructure engineering and defect engineering strategies are combined to improve the conductivity of IrO x / TiO2 activity and durability. In electrocatalytic systems, lattice stress strategies are widely used to regulate the d-band center displacement and optimize the intermediate binding performance. By preparing anatase and rutile two-phase structures as the carrier core, a three-phase heterostructure is formed after loading the shell iridium oxide. The process of lattice matching to form a heterostructure will produce lattice strain, distort the structure of TiO2, activate the O atoms near the active site as proton acceptors, reduce the energy barrier to form *OOH, and thus improve the OER activity. In addition, the Ti-O-Ir bridge structure at the anatase TiO2 interface provides a channel for electron transfer between Ti and Ir. Rutile TiO2 is conducive to serving as the core of iridium oxide, forming iridium oxide with a rutile structure, increasing the interaction between the core titanium oxide and iridium oxide, and thus improving the stability of iridium oxide. The sol-gel method has the advantages of low cost, simple preparation, and low pollution, and is an ideal method for manufacturing two-phase TiO2. The surface conditions are carefully adjusted by the parameters of the sol-gel method, calcination temperature, dopants and their concentrations, thereby regulating the ratio of anatase and rutile phases.

[0005] At present, PEM water electrolysis OER catalysts rely on iridium precious metal or iridium oxide. Due to the dissolution and leaching of iridium, electrocatalysts based on Ir or amorphous IrO2 are unstable in acidic electrolytes, and the utilization rate of iridium needs to be improved. Using titanium oxide as a carrier is an effective way to improve the utilization rate of iridium. However, the conventional preparation method has poor conductivity, large grain size, and small specific surface area, which limits the application of titanium oxide as an OER carrier. For example, commercial Ti n O 2n-7 Although the conductivity is increased, it has poor stability under high potential conditions of OER and is prone to form TiO2, which reduces the conductivity and thus reduces the performance of the OER catalyst. Summary of the invention

[0006] The embodiment of the present invention provides a heterogeneous structure titanium oxide supported oxide catalyst and its preparation method and application, aiming to solve the problem that the existing OER catalyst has poor stability under high potential conditions, is easy to form TiO2 to reduce conductivity, and thus reduces the performance of the OER catalyst. The present invention improves the utilization rate of iridium or ruthenium, OER catalytic activity and stability by preparing a low-iridium core-shell catalyst with a two-phase heterogeneous structure titanium oxide as the core; and improves the specific surface area and conductivity of nano-titanium oxide, and is used as an OER catalyst carrier.

[0007] The technical solution of the present invention is achieved in this way:

[0008] A method for preparing a heterogeneous structure titanium oxide supported oxide catalyst comprises the following steps:

[0009] S01: hydrolyzing a titanium-containing organic compound precursor in alcohol to prepare a first metal (m) atom-doped titanium oxide sol;

[0010] S02: drying the titanium oxide sol prepared in step S01 to obtain a titanium oxide gel;

[0011] S03: heat-treating the titanium oxide gel in step S02 to prepare a first metal-doped titanium oxide (m-TiO x );

[0012] S04: Loading the second metal oxide particles (MO x ); obtaining a heterogeneous structure titanium oxide supported oxide catalyst; wherein the second metal is at least one of Ir or Ru.

[0013] Furthermore, in step S01, the specific steps of hydrolysis are: adding nitric acid to isopropanol and mixing, then adding a titanium-containing organic compound precursor and a first metal nitrate, adding deionized water and mixing, and hydrolyzing for 6-24 hours. The reactants are fully mixed to obtain a titanium oxide sol doped with a first metal atom; wherein the nitric acid is 0.05-0.2vl.% of the isopropanol; the ratio of the concentration of the metal nitrate to the concentration of the titanium-containing organic precursor is 0.2%-1%; and the molar amount of the deionized water is 4-8 times the molar amount of titanium.

[0014] The nitric acid is concentrated nitric acid, and the concentration of nitric acid is 68%-72%.

[0015] The mixing in step S01 is preferably carried out by using magnetic stirring to fully mix.

[0016] The titanium-containing organic compound precursor in step S01 is preferably at least one of titanium tetraisopropoxide or n-butyl titanate. The concentration of the titanium-containing organic compound precursor is 0.05-0.3 mmol / L.

[0017] The first metal is preferably at least one of Al, Zn, Ni, Mn, W or Nb.

[0018] Wherein, vl.% is the volume percentage.

[0019] Furthermore, in step S02, the drying temperature is preferably 40-120°C, and the drying time is greater than or equal to 4 hours to obtain a gel.

[0020] Furthermore, in step S03, the atmosphere of the heat treatment is preferably an atmosphere containing more than 5% oxygen, the temperature of the heat treatment is preferably 500-800° C., the time of the heat treatment is preferably 1-4 hours, and finally the obtained product is fully ground to obtain the first metal-doped titanium oxide (m-TiO x ). Wherein, m is the first metal.

[0021] Furthermore, in step S04, the method of loading the second metal oxide particles on the surface of the first metal-doped titanium oxide obtained in step S03 is preferably a method of heat-treating and oxidizing after polyol reduction.

[0022] The specific method for the polyol reduction is: uniformly disperse the first metal-doped titanium oxide obtained in step S03 in an ethylene glycol aqueous solution, add a second metal precursor salt, the mass of the second metal accounts for 40wt.%-80wt.% of the total mass of the product, mix well, and then heat the mixture to 120°C-200°C, react for 30S-3min, wash and dry the product, and obtain a heterogeneous structure titanium oxide loaded with a second metal catalyst (M / m-TiO2).

[0023] Wherein, the volume fraction of ethylene glycol in the ethylene glycol aqueous solution is greater than or equal to 50%;

[0024] The concentration of the second metal is 0.2 mmol / L-3 mmol / L.

[0025] The mass of the second metal accounts for 40wt.%-80wt.% of the total mass of the product, specifically, the mass of the second metal divided by the mass of the second metal and the first metal doped titanium oxide (m-TiOx) is 40wt.%-80wt.%.

[0026] The method for fully mixing and homogenizing adopts at least one of the dispersion modes of ultrasound, stirring or cell disruption.

[0027] The second metal precursor salt is preferably at least one of iridium salts or ruthenium salts.

[0028] The mixture is preferably heated by microwave heating.

[0029] Further, the heat treatment oxidation conditions are: the heat treatment atmosphere is an oxygen-containing atmosphere greater than 5%, the heat treatment temperature is 300-550°C, the heat treatment time is 2-8h, and a heterogeneous structure titanium oxide supported oxide catalyst (MO x / m-TiO2).

[0030] The heat treatment oxidation is preferably carried out in a tube furnace.

[0031] A heterogeneous structure titanium oxide supported oxide catalyst is obtained by the above preparation method.

[0032] The heterogeneous structured titanium oxide-supported oxide catalyst is applied as an OER electrocatalyst in a proton exchange membrane water electrolyzer.

[0033] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0034] 1. In the preparation method of the heterogeneous structured titanium oxide supported oxide catalyst of the present invention, a sol-gel method is used to prepare a first metal heteroatom-doped two-phase heterogeneous titanium oxide as a core or carrier. The first metal heteroatom doping improves the conductivity of the titanium oxide. At the same time, the two-phase heterogeneous titanium oxide forms a heterogeneous structure with the OER active part on its surface, thereby improving the activity and durability of the catalyst.

[0035] 2. The present invention prepares a highly active and durable low iridium / ruthenium core-shell catalyst, improves the utilization rate of iridium / ruthenium, and reduces the amount of iridium / ruthenium used in the PEM water electrolysis anode.

[0036] 3. The two-phase structured titanium oxide prepared by the present invention is used as an OER catalyst carrier material.

[0037] 4. The heterogeneous structured titanium oxide supported oxide catalyst prepared by the present invention increases the specific surface area and electrical conductivity of nano-titanium oxide and is used as an OER catalyst carrier. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0040] At present, the existing OER catalysts have the disadvantages of poor stability under high potential conditions and easy formation of TiO2 to reduce conductivity, thereby reducing the performance of the OER catalyst. In order to solve the above technical problems, the present invention proposes a heterogeneous structure titanium oxide supported oxide catalyst and its preparation method and application.

[0041] Example 1

[0042] A method for preparing a heterogeneous titanium oxide supported iridium oxide catalyst, using a sol-gel method to prepare a Zn atom-doped two-phase heterogeneous titanium oxide as a core or carrier, metal heteroatom doping improves the conductivity of the titanium oxide, and the two-phase heterogeneous titanium oxide and the OER active part on its surface form a heterogeneous structure to improve the activity and durability of the catalyst; specifically comprising the following steps:

[0043] S01: preparing Zn metal atom-doped titanium oxide sol by hydrolyzing a titanium-containing organic compound precursor in alcohol;

[0044] S02: drying the Zn metal atom-doped titanium oxide sol prepared in step S01 to obtain titanium oxide gel;

[0045] S03: heat treating the titanium oxide gel in step S02 to prepare a two-phase heterogeneous structure of Zn-doped titanium oxide (Zn-TiO x );

[0046] S04: The surface of the Zn-doped titanium oxide with a two-phase heterogeneous structure obtained in step S03 is loaded with Ir metal oxide particles to obtain a heterogeneous structure titanium oxide loaded iridium oxide catalyst.

[0047] In step S01, the specific steps of the hydrolysis are: add 50ul nitric acid (commercially available concentrated nitric acid) to 57ml isopropanol, stir magnetically to mix thoroughly, then add titanium tetraisopropoxide precursor, the concentration of titanium tetraisopropoxide precursor is 0.1mmol / L; add zinc nitrate, the ratio of the molar amount of zinc nitrate to the molar amount of titanium tetraisopropoxide is 0.5%; add 1.9mL deionized water and stir magnetically for 12h to mix thoroughly, the molar amount of deionized water is 6 times the molar amount of titanium, the hydrolysis reaction time is 12h, ensure that the reactants are fully mixed, and obtain Zn metal atom-doped titanium oxide sol.

[0048] In step S02, the drying temperature is 80°C and the drying time is 4 hours to obtain a gel.

[0049] In step S03, the heat treatment atmosphere is air atmosphere, the heat treatment temperature is 600° C., the heat treatment time is 2 h, and finally the obtained product is fully ground to obtain Zn-doped anatase rutile two-phase heterogeneous titanium oxide.

[0050] In step S04, the method for loading Ir metal oxide particles on the surface of Zn-doped titanium oxide with a two-phase heterogeneous structure obtained in step S03 is a method of performing heat treatment oxidation after polyol reduction.

[0051] The specific method of polyol reduction is: the Zn-doped titanium oxide with two-phase heterogeneous structure obtained in step S03 is uniformly dispersed in an ethylene glycol aqueous solution, the volume fraction of ethylene glycol is 100%, and the precursor salt of metal Ir, chloroiridic acid, is added, the concentration of Ir metal is 0.15mmol / L, and the mass of Ir metal accounts for 75wt.% of the total mass of the product (i.e., the mass of Ir metal is divided by the mass of Ir metal and Zn-TiO x The mixture was mixed by ultrasonic, stirring and cell crushing to obtain a Zn-doped titanium oxide surface-loaded Ir metal particle catalyst (Ir / Zn-TiO x catalyst).

[0052] The heat treatment oxidation conditions are: the Ir / Zn-TiO x The catalyst was heat treated in a tube furnace in an air atmosphere at a temperature of 400°C for 4 h to obtain a heterogeneous Zn-doped titanium oxide supported iridium oxide catalyst (IrO x / Zn-TiO x catalyst).

[0053] The Zn-TiO obtained in step S03 xThe particle size is 8nm±0.5nm, with high conductivity and large specific surface area. x The Ir particle size range in the catalyst is 1.8-2.8nm, and the RDE test overpotential is 190mv@10mA / cm 2 The PEM electrolyzer test membrane electrode performance reached 1.52V@2A / cm 2 , after 1000h test, the attenuation is 32mV. Step S04: IrO x / Zn-TiO x IrO in catalyst x The particle size range is 3.5-4.8nm, and the RDE test overpotential is 250mv@10mA / cm 2 The PEM electrolyzer test membrane electrode performance reached 1.63V@2A / cm 2 , attenuated by 20mV after 1000h test.

[0054] Example 2

[0055] A method for preparing a heterogeneous titanium oxide supported iridium oxide catalyst, using a sol-gel method to prepare a Nb atom-doped two-phase heterogeneous titanium oxide as a core or carrier, metal heteroatom doping improves the conductivity of the titanium oxide, and the two-phase heterogeneous titanium oxide and the OER active part on its surface form a heterogeneous structure to improve the activity and durability of the catalyst; comprising the following steps:

[0056] S01: preparing Nb metal atom-doped titanium oxide gel by hydrolyzing a titanium-containing organic compound precursor in alcohol;

[0057] S02: drying the Nb metal atom-doped titanium oxide sol prepared in step S01 to obtain titanium oxide gel;

[0058] S03: heat treating the titanium oxide gel in step S02 to prepare a two-phase heterogeneous structure of Nb-doped titanium oxide (Nb-TiO x );

[0059] S04: The surface of the Nb-doped titanium oxide with a two-phase heterogeneous structure obtained in step S03 is loaded with Ir metal oxide particles to obtain a heterogeneous titanium oxide-loaded iridium oxide catalyst.

[0060] In step S01, the specific steps of the hydrolysis are: adding 50ul nitric acid (commercially available concentrated nitric acid) to 57ml isopropanol, stirring magnetically to mix thoroughly, and then adding titanium tetraisopropoxide precursor, the concentration of which is 0.1mmol / L; adding niobium nitrate, the ratio of the molar amount of niobium nitrate to the molar amount of titanium tetraisopropoxide precursor is 0.5%; adding 1.9mL deionized water and stirring magnetically for 12h to mix thoroughly, the molar amount of water is 6 times the molar amount of titanium, and the hydrolysis reaction time is 12h to ensure that the reactants are fully mixed to obtain titanium oxide gel doped with Nb metal atoms.

[0061] In step S02, the drying temperature is 80°C and the drying time is 5 hours to obtain a gel.

[0062] In step S03, the heat treatment atmosphere is air atmosphere, the heat treatment temperature is 700° C., the heat treatment time is 2 h, and finally the obtained product is fully ground to obtain Nb-doped anatase rutile two-phase heterogeneous titanium oxide.

[0063] In step S04, the method of loading Ir metal oxide particles on the surface of Nb-doped titanium oxide of the two-phase heterogeneous structure is a method of performing heat treatment oxidation after polyol reduction.

[0064] The specific method of polyol reduction is: uniformly dispersing the Nb doping oxidation of the two-phase heterogeneous structure obtained in step S03 in an ethylene glycol aqueous solution, wherein the volume fraction of ethylene glycol is 100%, adding iridic acid, a precursor salt of metal Ir, wherein the concentration of Ir metal is 0.15 mmol / L, and the mass of Ir metal accounts for 75 wt.% of the total mass of the product (i.e., the mass of Ir metal divided by the mass of Ir metal and Nb-TiO x The mixture was mixed by ultrasonic, stirring and cell crushing to obtain a Nb-doped titanium oxide surface-loaded Ir metal particle catalyst (Ir / Nb-TiO x catalyst).

[0065] The conditions for the heat treatment oxidation are: the above product Ir / Nb-TiO x As for the heat treatment in a tube furnace, the heat treatment atmosphere was air atmosphere, the heat treatment temperature was 400 ° C, and the heat treatment time was 4 h to obtain a heterogeneous structure Nb-doped titanium oxide supported iridium oxide catalyst (IrOx / Nb-TiO x catalyst).

[0066] The Nb-TiO obtained in step S03 xThe particle size is 9nm±0.5nm, with high conductivity and large specific surface area. x The Ir particle size range in the catalyst is 1.9-2.9nm, and the RDE test overpotential is 180mv@10mA / cm 2 , PEM electrolyzer test membrane electrode performance reached 1.50V@2A / cm 2 , after 1000h test, the attenuation is 30mV. Step S04: IrO obtained after heat treatment and oxidation x / Nb-TiO x IrO in catalyst x The particle size range is 3.5-4.8nm, and the RDE test overpotential is 240mv@10mA / cm 2 The PEM electrolyzer test membrane electrode performance reached 1.61V@2A / cm 2 , after 1000h test, it decays by 18mV.

[0067] Example 3

[0068] A method for preparing a heterogeneous titanium oxide supported ruthenium oxide catalyst, using a sol-gel method to prepare a Nb atom-doped two-phase heterogeneous titanium oxide as a core or carrier, metal heteroatom doping improves the conductivity of the titanium oxide, and the two-phase heterogeneous titanium oxide and the OER active part on its surface form a heterogeneous structure to improve the activity and durability of the catalyst; comprising the following steps:

[0069] S01: preparing Nb metal atom-doped titanium oxide gel by hydrolyzing a titanium-containing organic compound precursor in alcohol;

[0070] S02: drying the Nb metal atom-doped titanium oxide sol prepared in step S01 to obtain titanium oxide gel;

[0071] S03: heat treating the titanium oxide gel in step S02 to prepare a two-phase heterogeneous structure of Nb-doped titanium oxide (Nb-TiO x );

[0072] S04: Ru metal oxide particles are loaded on the surface of the Nb-doped titanium oxide with a two-phase heterogeneous structure obtained in step S03 to obtain a heterogeneous titanium oxide-loaded ruthenium oxide catalyst.

[0073] In step S01, the specific steps of the hydrolysis are: adding 50ul nitric acid (commercially available concentrated nitric acid) to 57ml isopropanol, stirring magnetically to mix thoroughly, and then adding titanium tetraisopropoxide precursor, the concentration of which is 0.1mmol / L; adding niobium nitrate, the ratio of the molar amount of niobium nitrate to the molar amount of titanium tetraisopropoxide precursor is 0.5%; adding deionized water and stirring magnetically for 12h to mix thoroughly, the molar amount of water is 6 times the molar amount of titanium, and the hydrolysis reaction time is 12h to ensure that the reactants are fully mixed to obtain titanium oxide gel doped with Nb metal atoms.

[0074] In step S02, the drying temperature is 80°C and the drying time is 6 hours to obtain a gel.

[0075] In step S03, the heat treatment atmosphere is air atmosphere, the heat treatment temperature is 700° C., the heat treatment time is 2 h, and finally the obtained product is fully ground to obtain Nb-doped anatase rutile two-phase heterogeneous titanium oxide.

[0076] In step S04, the method of loading Ru metal oxide particles on the surface of Nb-doped titanium oxide of the two-phase heterogeneous structure is a method of performing heat treatment oxidation after polyol reduction.

[0077] The specific method of polyol reduction is: uniformly dispersing the two-phase heterogeneous structure Nb-doped titanium oxide obtained in step S03 in an ethylene glycol aqueous solution, wherein the volume fraction of ethylene glycol is 100%, adding ruthenium trichloride, a precursor salt of metal Ru, wherein the concentration of Ru metal is 0.15 mmol / L, and the mass of Ru metal accounts for 75 wt.% of the total mass of the product (i.e., the mass of Ru metal divided by the mass of Ru metal and Nb-TiO x The mixture was mixed by ultrasonic, stirring and cell crushing to obtain a Ru metal particle catalyst with a two-phase heterogeneous structure of Nb-doped titanium oxide surface supported by Ru. x catalyst).

[0078] The heat treatment oxidation method is specifically: reducing the Ru / Nb-TiO x As for the heat treatment in the tube furnace, the atmosphere of the heat treatment was air atmosphere, the temperature of the heat treatment was 400°C, and the heat treatment time was 4 h. x / Nb-TiO x catalyst).

[0079] The Nb-TiO obtained in step S03 xThe particle size is 9nm±0.5nm, with high conductivity and large specific surface area. x The Ru particle size range in the catalyst is 1.9-2.9nm, and the RDE test overpotential is 168mv@10mA / cm 2 The PEM electrolyzer test membrane electrode performance reached 1.48V@2A / cm 2 , after 1000h test, the decay is 43mV. Step S04: RuO obtained after heat treatment and oxidation x / Nb-TiO x RuO in catalyst x The particle size range is 4-5nm, and the RDE test overpotential is 220mv@10mA / cm 2 The PEM electrolyzer test membrane electrode performance reached 1.57V@2A / cm 2 , after 1000h test, it decays by 32mV.

[0080] Comparative Example 1

[0081] A method for preparing a titanium oxide-supported iridium oxide catalyst comprises the following steps:

[0082] A polyol reduction method is adopted, specifically, commercial titanium oxide (TiO2) is uniformly dispersed in an ethylene glycol aqueous solution, the volume fraction of ethylene glycol is 100%, chloroiridic acid is added, the Ir metal concentration is 0.15 mmol / L, and the mass of Ir metal accounts for 75wt.% of the total mass of the product (that is, the mass of Ir metal divided by the sum of the mass of Ir metal and TiO2 is 75wt.%); the mixture is fully mixed by using an ultrasonic, stirring, and cell crushing dispersion method; the mixture is then heated to 160°C under microwave conditions and reacted for 120S; the product is washed and dried to obtain a titanium oxide-loaded iridium catalyst (Ir / TiO2 catalyst).

[0083] Further, the Ir / TiO2 catalyst was subjected to heat treatment oxidation. Specifically, the product Ir / TiO2 was subjected to heat treatment in a tube furnace. The heat treatment atmosphere was an air atmosphere. The heat treatment temperature was 400° C. and the heat treatment time was 4 h. Thus, a titanium oxide supported iridium oxide catalyst (IrO x / TiO x catalyst).

[0084] The particle size of commercial TiO2 is 20nm. The particle size of Ir in Ir / TiO2 catalyst ranges from 2-4nm, and the overpotential of RDE test is 380mv@10mA / cm 2 , PEM electrolyzer test membrane electrode performance reached 2.0V@2A / cm 2 , after 1000h test, the attenuation is 56mV. IrO obtained after heat treatment and oxidation x / TiO x IrO in catalyst x The particle size range is 4-5nm, and the RDE test overpotential is 390mv@10mA / cm 2 , PEM electrolyzer test membrane electrode performance reached 2.3V@2A / cm 2 , after 1000h test, it decays by 43mV.

[0085] By comparison, it can be seen that the catalytic performance of the heterogeneous structured titanium oxide supported iridium oxide / ruthenium oxide catalysts obtained in Examples 1 to 3 is much higher than that of the titanium oxide supported iridium oxide catalyst obtained in Comparative Example 1.

[0086] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0087] 1. In the preparation method of the heterogeneous structured titanium oxide supported oxide catalyst of the present invention, a sol-gel method is used to prepare a first metal heteroatom-doped two-phase heterogeneous titanium oxide as a core or carrier. The first metal heteroatom doping improves the conductivity of the titanium oxide. At the same time, the two-phase heterogeneous titanium oxide forms a heterogeneous structure with the OER active part on its surface, thereby improving the activity and durability of the catalyst.

[0088] 2. The present invention prepares a highly active and durable low-ruthenium / ruthenium core-shell catalyst, improves the utilization rate of iridium / ruthenium, and reduces the amount of iridium / ruthenium used in the PEM water electrolysis anode.

[0089] 3. The two-phase structured titanium oxide prepared by the present invention is used as an OER catalyst carrier material.

[0090] 4. The heterogeneous structured titanium oxide supported oxide catalyst prepared by the present invention increases the specific surface area and electrical conductivity of nano-titanium oxide and is used as an OER catalyst carrier.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a heterogeneous titanium oxide supported oxide catalyst, Features: The steps include: S01: hydrolyzing a titanium-containing organic compound precursor in alcohol to prepare a first metal atom-doped titanium oxide sol; S02: drying the titanium oxide sol prepared in step S01 to obtain a titanium oxide gel; S03: heat treating the titanium oxide gel in step S02 to prepare a first metal-doped titanium oxide with a two-phase heterogeneous structure; S04: Loading second metal oxide particles on the surface of the first metal-doped titanium oxide obtained in step S03; obtaining a heterogeneous structure titanium oxide-loaded oxide catalyst; wherein the second metal is at least one of Ir and Ru.

2. The method for preparing the heterogeneous titanium oxide supported oxide catalyst according to claim 1, Features: In step S01, the specific steps of hydrolysis are: adding nitric acid to isopropanol and mixing, then adding a titanium-containing organic compound precursor and a first metal nitrate, adding deionized water and mixing, and hydrolyzing for 6-24 hours. The reactants are fully mixed to obtain a titanium oxide sol doped with a first metal atom; wherein the nitric acid is 0.05-0.2vl.% of the isopropanol; the ratio of the concentration of the metal nitrate to the concentration of the titanium-containing organic precursor is 0.2%-1%; and the molar amount of the deionized water is 4-8 times the molar amount of titanium.

3. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 2, Features: In step S01, the titanium-containing organic compound precursor is at least one of titanium tetraisopropoxide or n-butyl titanate; The first metal is at least one of Al, Zn, Ni, Mn, W or Nb.

4. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 1, Features: In step S02, the drying temperature is 40-120°C, and the drying time is greater than or equal to 4 hours to obtain a gel.

5. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 1, Features: In step S03, the heat treatment atmosphere is an atmosphere containing more than 5% oxygen, the heat treatment temperature is 500-800°C, the heat treatment time is 1-4h, and finally the obtained product is fully ground to obtain a first metal-doped titanium oxide with a two-phase heterogeneous structure.

6. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 1, Features: In step S04, the method of loading the second metal oxide particles on the surface of the first metal-doped titanium oxide obtained in step S03 is a method of performing heat treatment oxidation after polyol reduction.

7. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 6, Features: The specific method of polyol reduction is: uniformly dispersing the first metal-doped titanium oxide obtained in step S03 in an ethylene glycol aqueous solution, adding a second metal precursor salt, wherein the mass of the second metal accounts for 40wt.%-80wt.% of the total mass of the product, and fully mixing, and then heating the mixture to 120°C-200°C, reacting for 30S-3min, washing and drying the product, and obtaining a heterogeneous structure titanium oxide-supported second metal catalyst; The second metal precursor salt is at least one of iridium salts or ruthenium salts.

8. The method for preparing the heterogeneous structured titanium oxide supported oxide catalyst according to claim 6, Features: The conditions of the heat treatment oxidation are: the heat treatment atmosphere is an oxygen-containing atmosphere greater than 5%, the heat treatment temperature is 300-550° C., and the heat treatment time is 2-8 hours, so as to obtain a heterogeneous structure titanium oxide supported oxide catalyst.

9. A heterogeneous structure titanium oxide supported oxide catalyst obtained by the preparation method according to any one of claims 1 to 8.

10. Application of the heterogeneous titanium oxide-supported oxide catalyst according to claim 9 as an OER electrocatalyst in a proton exchange membrane water electrolyzer.

Citation Information

Cited By

  • Titanium dioxide out-phase junction with controllable crystal phase ratio as well as preparation method and application of titanium dioxide out-phase junction

    CN120423598A