Anode catalyst for producing hydrogen by electrolyzing water and preparation method of anode catalyst

By using carbon nitride nanotubes to support iridium oxide in the anode catalyst for hydrogen production by electrolyzing water, a loose porous structure is formed, which solves the problem of large amount of iridium metal, improves catalytic activity and stability, and reduces costs.

CN118957653APending Publication Date: 2024-11-15SHENZHEN XIWAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410963899.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The amount of iridium metal is used in the existing anode catalysts for hydrogen production by electrolyzing water, resulting in high cost and insufficient catalytic activity and stability.

Method used

By using carbon nitride nanotubes as support, the iridium oxide is supported to form a loose porous structure, which improves the active area and stability of the catalyst and reduces the use of iridium metal.

Benefits of technology

The amount of iridium metal is reduced, catalytic activity and stability is improved, carbon loss is reduced, and the efficiency of hydrogen evolution reaction is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957653A_ABST
    Figure CN118957653A_ABST
Patent Text Reader

Abstract

The invention provides an anode catalyst for producing hydrogen by electrolyzing water and a preparation method thereof. The preparation method of the anode catalyst for producing hydrogen by electrolyzing water comprises the following steps: providing iridium oxide; preparing a carbon nano tube, and performing nitrogen doping on the carbon nano tube to obtain a carbon nitride nano tube; and loading the iridium oxide by using the carbon nitride nanotube to obtain the anode catalyst. According to the anode catalyst for hydrogen production by electrolysis of water and the preparation method thereof, the structure of the carrier carbon nanotube is optimized, active metal iridium oxide can be better loaded, and iridium oxide particles are dispersed to form more effective point locations, so that the usage amount of precious metal iridium in unit area of an anti-reverse membrane electrode is reduced, and the service life of the anode catalyst is prolonged. And meanwhile, the catalytic activity effect can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of hydrogen production by water electrolysis, and more specifically, relates to an anode catalyst for hydrogen production by water electrolysis and a preparation method thereof. Background Art

[0002] Water electrolysis uses water as raw material to produce hydrogen, and uses an electrolysis process to decompose water into hydrogen and oxygen. Water electrolysis has the advantages of simple process, no pollution, and high purity of the produced hydrogen. The current main water electrolysis hydrogen production solutions include alkaline water electrolysis technology, proton exchange membrane water electrolysis technology (PEM-Proton Exchange Membrane Electrolysis), anion exchange membrane water electrolysis technology, and solid oxide water electrolysis technology. Proton exchange membrane water electrolysis technology exhibits the advantages of fast response, flexible load current, and pure hydrogen production. In specific application scenarios (such as automotive-grade hydrogen energy and volatile renewable energy), the advantages of proton exchange membrane water electrolysis technology are becoming increasingly obvious and have received widespread attention.

[0003] At present, the cathode and anode catalysts of water electrolysis membrane electrodes in commercial PEM are platinum and iridium-based nanomaterials, respectively. Among them, the catalytic activity and stability of the iridium-based catalyst on the oxygen evolution side play a vital role in the efficiency and service life of the membrane electrode. 2 Used as anode catalyst for PEM electrolysis, its particle size is large, resulting in slow oxygen evolution reaction kinetics and low mass activity. 2 The methods include melting method, impregnation thermal decomposition method and sol-gel method. The first two methods mainly dissolve the iridium precursor and polymer in the solution, and then prepare IrO by high temperature thermal decomposition in air. 2 The sol-gel method first prepares Ir and Ir(OH) 2 The colloidal particles were then calcined in air to obtain IrO 2 In the sol-gel method, iridium often exists in the form of a single metal, unlike platinum and palladium, which are usually loaded on a carrier. As a result, Ir nanoparticles are prone to agglomeration without adding a dispersant. In addition, when preparing the anode catalyst, iridium oxide metal is directly coated on the surface of the substrate, and the amount of iridium metal used is relatively large.

[0004] In summary, the current anode catalyst uses a large amount of metallic iridium, resulting in high costs. Summary of the invention

[0005] The purpose of the embodiments of the present application is to provide an anode catalyst for producing hydrogen by electrolysis of water and a preparation method thereof, so as to solve the technical problem that the amount of metal iridium used in the previous anode catalyst is relatively large.

[0006] To achieve the above objectives, the first aspect of the present application provides a method for preparing an anode catalyst for electrolyzing water to produce hydrogen, comprising:

[0007] Providing iridium oxide;

[0008] preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes;

[0009] The carbon nitride nanotubes are used to load the iridium oxide to obtain the anode catalyst.

[0010] The preparation method provided in the first aspect of the embodiment of the present application utilizes carrier carbon nanotubes, and by nitrogen doping the carbon nanotubes, the structure of the carbon nanotubes is transformed (a loose and porous mesh structure is obtained), so that the nitrided carbon nanotubes can fully load iridium oxide, and through the loading process, the active iridium oxide particles with small particle size and uniform dispersion are obtained. In this way, the available electrochemical surface area of ​​the hydrogen evolution reaction can be increased and the carbon loss during operation can be reduced. The iridium oxide particles are dispersed to form more effective points, thereby reducing the use of the precious metal iridium per unit area of ​​the anti-reverse polar membrane electrode, while ensuring the catalytic activity effect. The anode catalyst provided in the embodiment of the present application can greatly reduce the amount of iridium metal used, and improve the activity and stability of the iridium oxide catalyst.

[0011] Optionally, the step of preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes comprises:

[0012] Providing a layered catalyst with a metal supported on a carrier;

[0013] The atmosphere of carbon source and nitrogen source is introduced into the layered catalyst to react and obtain nitrided carbon nanotubes.

[0014] Preferably, the step of introducing an atmosphere of a carbon source and a nitrogen source into the layered catalyst to react and obtain nitrided carbon nanotubes comprises:

[0015] The first carbon source gas is introduced into the layered catalyst by a fluidized bed process to perform a first catalytic reaction to obtain initial carbon nanotubes attached to the surface of the layered catalyst, and then a second carbon source gas and a nitrogen source gas are introduced to perform a second catalytic reaction to obtain the nitrided carbon nanotubes. Thus, the influence of oxygen on the catalytic metal can be effectively avoided, the smooth growth of the carbon nanotubes is ensured, and the nitrogen doping is completed.

[0016] Preferably, before the carbon source and nitrogen source atmosphere are introduced into the layered catalyst to react and obtain nitrided carbon nanotubes, the process includes: reducing and activating the layered catalyst to obtain an activated catalyst. Thus, after the layered catalyst is reduced and activated, the catalytically active component (metal) of the catalyst has a stronger adsorption capacity on the carrier and an ion exchange capacity with the carrier; the catalytically active component elements are more easily introduced into the mesopores and micropores on the inner surface of the layered carrier material; the active elements can be evenly dispersed, and the loading amount and uniformity of the catalyst are increased. In the process of catalytic carbon nanotube growth, the carbon source can be evenly attached to the catalyst surface, and carbon nanotubes are grown under the catalytic action of the active elements; at the same time, nitrogen is inserted to obtain nitrogen-doped carbon nanotubes. This preparation method is suitable for fluidized bed production processes and can be used for industrial production.

[0017] Optionally, in the step of the first catalytic reaction:

[0018] The flow rate of the first carbon source gas is 500L / min to 600L / min. Optionally, the time of the first catalytic reaction is 8min to 15min. A high flow rate helps the carbon source gas to have good contact with the catalyst and promotes the growth of carbon nanotubes.

[0019] Optionally, in the step of the second catalytic reaction:

[0020] The flow rate of the second carbon source gas is 400L / min to 500L / min. Optionally, the flow rate of the nitrogen source gas is 50L / min to 100L / min. Slightly lower than the flow rate in the first catalytic reaction, it is beneficial to control the doping of nitrogen. Optionally, the time of the second catalytic reaction is 30min to 40min. A longer residence time may help to more fully dope the nitrogen element, which is beneficial to optimize the structure of the carbon nanotubes.

[0021] Optionally, the first carbon source gas and the second carbon source gas include at least one of cyclohexanone and cyclohexane. Optionally, the nitrogen source gas is ammonia.

[0022] Optionally, the lamellar catalyst is a vermiculite-supported metal catalyst, and specifically, the supported metal may include iron, cobalt, nickel, aluminum, etc. By using the lamellar catalyst, the surface area of ​​the catalyst carrier can be effectively utilized, so that the activated metal elements are evenly dispersed, thereby increasing the loading amount and uniformity of the catalyst, so that the carbon nanotubes can evenly adhere to the catalyst surface and grow.

[0023] Optionally, the step of using the carbon nitride nanotubes to load the iridium oxide to obtain the anode catalyst comprises:

[0024] providing a first solvent and an emulsifier;

[0025] The iridium oxide, the first solvent and the emulsifier are mixed by ultrasound, and then subjected to a first high-pressure homogenization to obtain a first mixture;

[0026] The carbon nitride nanotubes are added to the first mixture, and a second high-pressure homogenization is performed to obtain the anode catalyst. Physical means (such as ultrasound and high-pressure homogenization) are fully utilized to improve the dispersion and mixing uniformity of the carbon nanotubes, thereby improving the catalytic activity and stability of the finally formed anode catalyst.

[0027] Preferably, after the second high-pressure homogenization and before obtaining the anode catalyst, ultrasonic treatment, drying and grinding are sequentially performed to ensure the consistency of the particle size of the obtained anode catalyst for subsequent application.

[0028] Optionally, before the iridium oxide is loaded by carbon nitride nanotubes, the carbon nitride nanotubes are subjected to acid washing to remove impurities of the carbon nitride nanotubes and functional groups are introduced on the surface of the carbon nitride nanotubes to improve the activity and dispersibility of the carbon nitride nanotubes.

[0029] Preferably, the pickling treatment comprises:

[0030] Dispersing the carbon nitride nanotubes using an organic solvent;

[0031] Using a first solvent for washing and filtering;

[0032] A mixed acid solution is used for pickling and post-treatment.

[0033] In this way, impurities (metals, catalysts, etc.) on the carbon nanotubes can be effectively removed and hydrophilic functional groups can be introduced on the surface of the carbon nanotubes to improve their hydrophilicity and surface activity.

[0034] Optionally, the iridium oxide is purchased from the market, or prepared by the following steps, and the preparation of the iridium oxide includes:

[0035] Providing chloroiridic acid, ethylene glycol, and acid solution; iridium hexachloride, which is usually used as a source of iridium, and ethylene glycol as a reducing agent to help reduce iridium from its oxidized state to the metallic state;

[0036] After the chloroiridic acid and the ethylene glycol are mixed, the reaction is carried out in an oil bath; the oil bath provides a stable heating environment and can accurately control the reaction temperature;

[0037] After the reaction is completed, an acid solution is added to precipitate iridium. Adding an acid solution to the system will cause the precipitation of metallic iridium. The addition of the acid solution can change the pH value of the solution, causing the iridium to precipitate in a water-insoluble form.

[0038] The iridium single substance is heat-treated in an oxygen atmosphere to obtain the iridium oxide.

[0039] A second aspect of an embodiment of the present application provides an anode catalyst for use in catalytic water electrolysis to produce hydrogen technology. The anode catalyst is prepared using the preparation method described in the first aspect, and the anode catalyst has a mesh-like porous structure.

[0040] In the second aspect of the embodiment of the present application, the anode catalyst uses carbon nitride nanotubes as a carrier and iridium oxide as an active substance. The carbon nitride nanotubes themselves also have certain catalytic activity, so they can accelerate the hydrogen evolution reaction. Since the carbon nanotubes are nitrogen-doped, a looser mesh porous structure is formed, which increases the active area on the one hand and facilitates the rapid transfer of electrons and the rapid precipitation of gases on the other hand. In addition, the carbon surface electronic state is adjusted and optimized by nitrogen doping, further improving its catalytic activity. Carbon nitride nanotubes can better load the active metal iridium oxide, and the iridium oxide particles are dispersed to form more effective points, thereby reducing the use of the precious metal iridium in the unit area of ​​the anti-reverse polar membrane electrode, while ensuring the catalytic activity effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0042] Figure 1 A schematic flow chart of a method for preparing an anode catalyst for producing hydrogen by electrolysis of water provided in an embodiment of the present application. DETAILED DESCRIPTION

[0043] In the following description, specific details such as specific system structures, technologies, etc. are provided for the purpose of illustration rather than limitation, so as to provide a thorough understanding of the embodiments of the present application. However, it should be clear to those skilled in the art that the present application may also be implemented in other embodiments without these specific details. In other cases, detailed descriptions of well-known systems, devices, circuits, and methods are omitted to prevent unnecessary details from obstructing the description of the present application.

[0044] It should also be understood that the term “and / or” used in the specification and appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0045] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0046] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0047] In addition, in the description of the present application specification and the appended claims, the terms "first", "second", "third", etc. are only used to distinguish the descriptions and cannot be understood as indicating or implying relative importance.

[0048] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the statements "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. that appear in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways. "Multiple" means two or more.

[0049] The present application provides a method for preparing an anode catalyst for producing hydrogen by electrolysis of water, such as Figure 1 As shown, including:

[0050] S10, providing iridium oxide;

[0051] S20, preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes;

[0052] S30, using carbon nitride nanotubes to load iridium oxide to obtain an anode catalyst.

[0053] In the embodiment of the present application, the carrier carbon nanotube is used, and the structure of the carbon nanotube is transformed (a loose and porous mesh structure is obtained) by nitrogen doping the carbon nanotube, so that the nitrided carbon nanotube can fully load the iridium oxide, and through the loading process, the active iridium oxide particles with a small particle size and uniform dispersion are obtained. In this way, the available electrochemical surface area of ​​the hydrogen evolution reaction can be increased and the carbon loss during the operation can be reduced. The iridium oxide particles are dispersed to form more effective points, thereby reducing the usage of the precious metal iridium in the unit area of ​​the anti-reverse polar membrane electrode, while ensuring the catalytic activity effect. The anode catalyst provided by the embodiment of the present application can greatly reduce the usage of the iridium metal, and improve the activity and stability of the iridium oxide catalyst.

[0054] In the application, the order of S10 and S20 is not limited, that is, S10 can be performed first, S20 can also be performed first, or S10 and S20 can be performed simultaneously.

[0055] In some embodiments, in step S10, iridium oxide can be directly purchased from the market. In other embodiments, in step S10, iridium oxide is prepared by the following steps:

[0056] S11, providing chloroiridic acid, ethylene glycol and acid solution;

[0057] S12, mixing chloroiridic acid and ethylene glycol, and reacting them in an oil bath;

[0058] S13, after the reaction is completed, acid solution is added to precipitate to obtain iridium element;

[0059] S14, heat-treating iridium in an oxygen atmosphere to obtain iridium oxide. Thus, chloroiridic acid is usually used as a source of iridium, and ethylene glycol is used as a reducing agent to help reduce iridium from its oxidized state to a metallic state; the oil bath provides a stable heating environment and can accurately control the reaction temperature; adding acid to the system will cause the precipitation of metallic iridium, and the addition of acid can change the pH value of the solution, causing iridium to precipitate in a water-insoluble form.

[0060] In some embodiments, the concentration of metallic iridium in the polyol is 1 g / L to 2 g / L. The concentration of metallic iridium in the polyol should be within the above range. If the concentration is too high, it will lead to insufficient reduction of iridium and cause loss of raw materials. If the concentration is too low, it will lead to too little catalyst prepared in each batch, which will waste raw materials and lack economic value.

[0061] In application, the reaction temperature is between 170°C and 180°C, and the reaction time is between 2h and 4h. In some preferred embodiments, the reaction temperature is 175°C, and the reaction time is 3h. In step S13, the acid solution includes nitric acid, sulfuric acid, etc. After step S13 and before step S14, after the iridium element is precipitated, it is filtered, washed, and dried to obtain small-sized iridium element particles. In this way, it is convenient to oxidize in the next step to generate iridium oxide, and obtain iridium oxide of uniform size.

[0062] In some embodiments, S20, preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes comprises:

[0063] S21, providing a layered catalyst having a carrier-supported metal;

[0064] S22, introducing an atmosphere of a carbon source and a nitrogen source into the layered catalyst to react and obtain nitrided carbon nanotubes.

[0065] In step S21, the lamellar catalyst is a vermiculite-supported metal catalyst, and specifically, the metal supported may include metals such as iron, cobalt, nickel, and aluminum. In certain embodiments, the metal may include nickel, cobalt, and iron, and the corresponding vermiculite-supported metal catalyst is represented by "FeCoNi / vermiculite". In other embodiments, other lamellar catalysts or layered catalysts may also be used, such as catalyst FeCoAl / vermiculite, etc. The above catalysts may be purchased directly from the market or prepared by themselves. By using the above-mentioned lamellar catalyst, the surface area of ​​the catalyst carrier may be effectively utilized, so that the activated metal elements are evenly dispersed, thereby increasing the loading amount and uniformity of the catalyst, so that the carbon nanotubes can be evenly attached to the catalyst surface for growth.

[0066] In some embodiments, before step S22, the step of reducing and activating the layered catalyst includes:

[0067] The layered catalyst is placed in an atmosphere containing hydrogen and nitrogen to perform a reduction reaction, wherein:

[0068] The volume ratio of hydrogen to nitrogen is (1-2): 1. In this atmosphere, the lamellar catalyst can be fully reduced and activated. In some embodiments, the reduction reaction time is 5 min to 10 min. In some embodiments, the reduction reaction temperature is 300° C. to 400° C.

[0069] Specifically, the layered catalyst was added to the catalyst reduction activation device, and 100 L / min of hydrogen and nitrogen were introduced into the reduction activation device, the volume ratio of hydrogen to nitrogen was 1:1, the reduction reaction time was 5 min, and the reduction reaction temperature was 300°C. 2 / N 2Pre-reduction in the mixed atmosphere activates the lamellar catalyst. In other embodiments, the volume ratio of hydrogen to nitrogen can be 2:1, the reduction reaction time is 7 minutes, 8 minutes or 10 minutes, and the reduction reaction temperature is 350°C, 380°C or 400°C.

[0070] In some embodiments, S22, introducing an atmosphere of a carbon source and a nitrogen source into the layered catalyst to react to obtain nitrided carbon nanotubes comprises:

[0071] The first carbon source gas is introduced into the layered catalyst by a fluidized bed process to perform a first catalytic reaction to obtain initial carbon nanotubes attached to the surface of the catalyst, and then a second carbon source gas and a nitrogen source gas are introduced to perform a second catalytic reaction to obtain nitrided carbon nanotubes. In this way, the influence of oxygen on the catalytic metal can be effectively avoided, the smooth growth of carbon nanotubes is ensured, and nitrogen doping is completed.

[0072] In other embodiments, in step S22, the step of introducing the atmosphere of the carbon source and the nitrogen source into the activated catalyst to react and obtain the nitrided carbon nanotubes comprises:

[0073] A first carbon source gas is introduced into the activated catalyst by a fluidized bed process to perform a first catalytic reaction to obtain initial carbon nanotubes attached to the catalyst surface, and then a second carbon source gas and a nitrogen source gas are introduced to perform a second catalytic reaction to obtain nitrided carbon nanotubes.

[0074] Specifically, the fluidized bed process can be implemented by a fluidized bed reactor, such as placing the activated catalyst in a fluidized bed reactor to perform the fluidized bed process. For example, the activated catalyst is placed in a reaction vessel; the first carbon source gas is introduced into the reaction vessel to perform a first catalytic reaction to obtain initial carbon nanotubes attached to the surface of the activated catalyst, and then the second carbon source gas and the nitrogen source gas are introduced simultaneously to perform a second catalytic reaction to obtain nitrided carbon nanotubes.

[0075] In the application, the first carbon source gas and the second carbon source gas include at least one of cyclohexanone or cyclohexane. Since cyclohexane has a high degree of saturation, the carbon-carbon bond therein is difficult to break, so nitrogen is not easily inserted therein; in some embodiments, the first carbon source gas and the second carbon source gas are preferably cyclohexanone, and the carbon-oxygen bond in cyclohexanone is easier to break than the carbon-carbon bond, so nitrogen is easily inserted therein. The nitrogen source gas is ammonia.

[0076] In application, the catalytic reaction is carried out twice, because it is not easy to dope nitrogen into carbon nanotubes, and it is necessary to avoid the influence of oxygen (when cyclohexanone is selected as the carbon source, the carbon-oxygen bond is broken, and the oxygen in it will make the catalyst inactive after contacting with the catalyst) on the catalytic metal. Therefore, in the first catalytic reaction, only the carbon source is introduced, and part of the carbon source is first allowed to catalytically grow on the catalyst surface to grow carbon nanotubes; then the carbon source and nitrogen source are introduced at the same time, while the carbon nanotubes continue to grow, the nitrogen source is prevented from directly contacting the catalyst surface, thereby preventing the catalyst from being oxidized and losing its catalytic effect.

[0077] In some embodiments, the reaction vessel is a two-stage reactor connected in series, having a primary reactor and a secondary reactor; specifically, a carbon source is first introduced into the primary reactor to carry out a first catalytic reaction to obtain initial carbon nanotubes attached to the surface of the layered catalyst, and then a carbon source and a nitrogen source are simultaneously introduced into the secondary reactor to carry out a second catalytic reaction to obtain nitrided carbon nanotubes.

[0078] In some embodiments, in the first catalytic reaction step:

[0079] The flow rate of the first carbon source gas is 500 L / min to 600 L / min. In some embodiments, the time of the first catalytic reaction is 8 min to 15 min. In some embodiments, the temperature of the first catalytic reaction is 660° C. to 700° C.

[0080] In some embodiments, in the second catalytic reaction step:

[0081] The flow rate of the second carbon source gas is 400L / min to 500L / min. In some embodiments, the flow rate of the nitrogen source gas is 50L / min to 100L / min. In some embodiments, the time of the second catalytic reaction is 30min to 40min. In some embodiments, the temperature of the second catalytic reaction is 600℃ to 650℃.

[0082] In the application, by comparing the conditions of the first catalytic reaction and the second catalytic reaction, it is not difficult to see that the flow rate of the first carbon source gas in the first catalytic reaction is faster than the flow rate of the second carbon source gas in the second catalytic reaction; the reaction time in the first catalytic reaction is shorter than the second catalytic reaction time; the reaction temperature in the first catalytic reaction is higher than the temperature of the second catalytic reaction. This is because, in the first catalytic reaction, carbon nanotubes need to grow on the surface of the activated catalyst, which requires a higher temperature and more carbon source gas; after a few minutes, once the carbon nanotubes begin to grow, there is no need to introduce too much carbon source; the focus of the second catalytic reaction is to complete the insertion of nitrogen and the continued growth of carbon nanotubes.

[0083] In some embodiments, the first carbon source gas, the second carbon source gas, the nitrogen source gas, and the catalyst are introduced into the reaction vessel by an inert gas, wherein the inert gas includes helium, argon, xenon, etc. Specifically, in the first catalytic reaction, the flow rate of the inert gas is 550L / min to 650L / min; in the second catalytic reaction, the flow rate of the inert gas is 550L / min to 600L / min.

[0084] In some embodiments, the inert gas is used to deliver the catalyst, the first carbon source gas, the second carbon source gas, and the nitrogen source gas by continuous input or pulse input.

[0085] In some embodiments, S30, using the carbon nitride nanotubes to load the iridium oxide to obtain the anode catalyst comprises:

[0086] S31, providing a first solvent and an emulsifier;

[0087] S32, mixing iridium oxide, the first solvent and the emulsifier by ultrasonication, and then performing a first high-pressure homogenization to obtain a first mixture;

[0088] S33, adding carbon nitride nanotubes to the first mixture, and performing a second high-pressure homogenization to obtain an anode catalyst.

[0089] Physical means (such as ultrasound and high-pressure homogenization) are fully utilized to improve the dispersion and mixing uniformity of carbon nanotubes, thereby improving the catalytic activity and stability of the final anode catalyst.

[0090] In step S31, the first solvent includes but is not limited to deionized water, distilled water, ultrapure water, etc.; the emulsifier includes but is not limited to OP-4, OP-7, OP-10, OP-15, OP-20, etc. In some embodiments, the emulsifier is preferably OP-10, which is a kind of alkylphenol polyoxyethylene ether (Alkylphenol Ethoxylate), specifically octylphenol polyoxyethylene ether (Octylphenol Ethoxylate), which belongs to non-ionic surfactant. This type of emulsifier has good emulsification, wetting, diffusion and antistatic properties.

[0091] In step S32, 1 g of iridium oxide, 20 g of deionized water and 0.1 g of emulsifier OP-10 were mixed and ultrasonicated for 30 min, and then high-pressure homogenization was performed using an ultra-high pressure homogenizer, wherein the turbulent pressure was 20 MPa, the time was 40 min, and the slurry volume circulation flow rate was 120 ml / min. The purpose of the first high-pressure homogenization is to allow the iridium oxide to be fully dispersed, and then fully contacted and mixed with the carbon nitride nanotubes during the second high-pressure homogenization.

[0092] Preferably, after the second high-pressure homogenization and before obtaining the anode catalyst, ultrasonic treatment, drying and grinding are sequentially performed to ensure the consistency of the particle size of the obtained anode catalyst for subsequent application.

[0093] In some embodiments, before step S30, the process includes: performing an acid wash treatment on the carbon nitride nanotubes to remove impurities in the carbon nitride nanotubes and introducing functional groups on the surfaces of the carbon nitride nanotubes to improve the activity and dispersibility of the carbon nitride nanotubes.

[0094] Therefore, acid washing of carbon nitride nanotubes has the following beneficial effects: First, it can remove metal catalyst residues: In the process of synthesizing carbon nanotubes, metal catalysts such as iron, nickel, cobalt, etc. are often used. Acid washing can effectively remove these metal residues to prevent them from causing adverse effects in subsequent applications, such as catalytic side reactions or reducing the electrochemical properties of the material. Second, it improves dispersibility: acid washing can introduce hydrophilic functional groups such as carboxyl (-COOH) or hydroxyl (-OH) to the surface of carbon nanotubes, which helps to improve the dispersibility of carbon nanotubes in water or polar organic solvents and makes iridium oxide easier to mix with them. Third, it reduces aggregation: carbon nanotubes tend to aggregate to form bundle structures, which will affect their distribution and performance in composite materials. Acid washing can break some tube bundles, reduce aggregation, and improve the separation of single carbon nanotubes.

[0095] In some embodiments, the pickling treatment includes:

[0096] The carbon nitride nanotubes are dispersed by using an organic solvent;

[0097] Using a first solvent for washing and filtering;

[0098] A mixed acid solution is used for pickling and post-treatment.

[0099] In this way, impurities (metals, catalysts, etc.) on the carbon nanotubes can be effectively removed and hydrophilic functional groups can be introduced on the surface of the carbon nanotubes to improve their hydrophilicity and surface activity.

[0100] In some embodiments, the organic solvent includes but is not limited to n-butanol, n-pentanol, isobutanol, ethanol, propanol, ether, etc. The first solvent includes but is not limited to deionized water, and the mixed acid solution includes a mixed solution of sulfuric acid and nitric acid. In a preferred embodiment, the mixed acid solution is sulfuric acid and nitric acid in a molar ratio of 1:1, with a total concentration of 5 mol / L.

[0101] An embodiment of the present application further provides an anode catalyst for producing hydrogen by electrolysis of water. The anode catalyst is prepared by the preparation method described in the first aspect, and the anode catalyst has a mesh-like porous structure.

[0102] In the second aspect of the embodiment of the present application, the anode catalyst uses carbon nitride nanotubes as a carrier and iridium oxide as an active substance. The carbon nitride nanotubes themselves also have a certain catalytic activity, so they can accelerate the hydrogen evolution reaction. Since the carbon nanotubes are nitrogen-doped, a looser mesh porous structure is formed, which increases the active area on the one hand and facilitates the rapid transfer of electrons and the rapid precipitation of gases on the other hand. In addition, the carbon surface electronic state is adjusted and optimized by nitrogen doping, which further improves its catalytic activity.

[0103] Carbon nitride nanotubes can better load the active metal iridium oxide, and the iridium oxide particles are dispersed to form more effective points, thereby reducing the use of precious metal iridium per unit area of ​​the anti-reverse electrode membrane electrode, while ensuring the catalytic activity effect.

[0104] The following provides specific examples for illustration.

[0105] Example 1

[0106] The present invention provides a method for preparing an anode catalyst for producing hydrogen by electrolysis of water, comprising the following steps:

[0107] S10, providing iridium oxide;

[0108] S11, providing 10 ml of 0.4% by mass chloroiridic acid solution, 50 ml of ethylene glycol and nitric acid;

[0109] S12, mixing the above chloroiridic acid and ethylene glycol, and reacting them in an oil bath at a reaction temperature of 175° C. and a reaction time of 3 h;

[0110] S13, after the reaction is completed, nitric acid is added to lower the pH of the system to 2, and iridium is precipitated;

[0111] S14, iridium single substance oxidation is heat-treated at 1000° C. in an oxygen atmosphere to obtain iridium oxide;

[0112] S20, preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes;

[0113] S21, providing a vermiculite-supported iron salt catalyst;

[0114] S22, introducing an atmosphere of a carbon source and a nitrogen source into the vermiculite-supported iron salt catalyst to react and obtain nitrided carbon nanotubes;

[0115] Specifically: the vermiculite-supported iron salt catalyst is transported to the reactor by inert gas, and the reactor is a two-stage reactor in series; the gas flow rate of the first reactor is 550 L / min of cyclohexane and 600 L / min of inert gas, the reaction temperature is 680°C, and the reaction time is 10 minutes from the entry of cyclohexane to the final discharge; the gas flow rate of the second reactor is 450 L / min of cyclohexane, 80 L / min of ammonia and 550 L / min of inert gas, the reaction temperature is 650°C, and the reaction time is 35 minutes from the entry of the carbon source to the final discharge;

[0116] Pickling treatment:

[0117] 2g of carbon nitride nanotubes and 150ml of n-butanol were mixed and stirred at room temperature for 1 hour, filtered and washed with deionized water for 3 times, 100ml of sulfuric acid and nitric acid solution (sulfuric acid and nitric acid in molar ratio of 1:1, total concentration of 5mol / L) were added to the filtered carbon nanotubes, refluxed and stirred at 90°C for 2h, and finally filtered and washed 5 times, dried in an oven at 60°C, and ground for use;

[0118] S30, using carbon nitride nanotubes to load iridium oxide to obtain an anode catalyst;

[0119] S31, take 1g of iridium oxide, 20g of deionized water and 0.1g of emulsifier OP-10;

[0120] S32, mixing iridium oxide, deionized water and an emulsifier by ultrasonication for 30 minutes, and then using an ultra-high pressure homogenizer for high pressure homogenization to obtain a first mixture, wherein the turbulent pressure is 20 MPa, the time is 40 min, and the slurry volume circulation flow rate is 120 ml / min;

[0121] S33. Then, 1 g of acid-washed carbon nitride nanotubes is added to the first mixture for a second high-pressure homogenization, wherein the turbulent pressure is 10 MPa, the time is 30 min, and the slurry volume circulation flow rate is 50 ml / min; finally, low-temperature ultrasound is applied at 5°C for 30 minutes, and then the mixture is dried in an oven at 60°C and ground for standby use to obtain the anode catalyst.

[0122] Example 2

[0123] S10, providing iridium oxide;

[0124] S11, providing 10 ml of 0.5% by mass chloroiridic acid solution, 50 ml of ethylene glycol and nitric acid;

[0125] S12, mixing the above chloroiridic acid and ethylene glycol, and reacting them in an oil bath at a reaction temperature of 175° C. and a reaction time of 3 h;

[0126] S13, after the reaction is completed, nitric acid is added to lower the pH of the system to 2, and iridium is precipitated;

[0127] S14, iridium single substance oxidation is heat-treated at 1000° C. in an oxygen atmosphere to obtain iridium oxide;

[0128] S20, preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes;

[0129] S21, providing a vermiculite-supported iron salt catalyst;

[0130] S22, introducing an atmosphere of a carbon source and a nitrogen source into the vermiculite-supported iron salt catalyst to react and obtain nitrided carbon nanotubes;

[0131] Specifically: the vermiculite-supported iron salt catalyst is transported to the reactor by inert gas, and the reactor is a two-stage reactor in series; the gas flow rate of the first reactor is 500 L / min of cyclohexane and 550 L / min of inert gas, the reaction temperature is 670°C, and the reaction time is 12 minutes from the entry of cyclohexane to the final discharge; the gas flow rate of the second reactor is 500 L / min of cyclohexane, 100 L / min of ammonia and 600 L / min of inert gas, the reaction temperature is 650°C, and the reaction time is 30 minutes from the entry of the carbon source to the final discharge;

[0132] Pickling treatment:

[0133] 2g of carbon nitride nanotubes and 150ml of n-butanol were mixed and stirred at room temperature for 1 hour, filtered and washed with deionized water for 3 times, 100ml of sulfuric acid and nitric acid solution (sulfuric acid and nitric acid in molar ratio of 1:1, total concentration of 5mol / L) were added to the filtered carbon nanotubes, refluxed and stirred at 90°C for 2h, and finally filtered and washed 5 times, dried in an oven at 60°C, and ground for use;

[0134] S30, using carbon nitride nanotubes to load iridium oxide to obtain an anode catalyst;

[0135] S31, take 1g of iridium oxide, 20g of deionized water and 0.1g of emulsifier OP-10;

[0136] S32, mixing iridium oxide, deionized water and an emulsifier by ultrasonication for 30 minutes, and then using an ultra-high pressure homogenizer for high pressure homogenization to obtain a first mixture, wherein the turbulent pressure is 20 MPa, the time is 40 min, and the slurry volume circulation flow rate is 120 ml / min;

[0137] S33. Then, 1 g of acid-washed carbon nitride nanotubes is added to the first mixture for a second high-pressure homogenization, wherein the turbulent pressure is 10 MPa, the time is 30 min, and the slurry volume circulation flow rate is 50 ml / min; finally, low-temperature ultrasound is applied at 5°C for 30 minutes, and then the mixture is dried in an oven at 60°C and ground for standby use to obtain the anode catalyst.

[0138] Example 3

[0139] S10, providing iridium oxide;

[0140] S11, providing 10 ml of 0.6% by mass chloroiridic acid solution, 70 ml of ethylene glycol and ml of nitric acid;

[0141] S12, mixing the above chloroiridic acid and ethylene glycol, and reacting them in an oil bath at a reaction temperature of 175° C. and a reaction time of 3 h;

[0142] S13, after the reaction is completed, nitric acid is added to lower the pH of the system to 2, and iridium is precipitated;

[0143] S14, iridium single substance oxidation is heat-treated at 1000° C. in an oxygen atmosphere to obtain iridium oxide;

[0144] S20, preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes;

[0145] S21, providing a vermiculite-supported iron salt catalyst;

[0146] S22, introducing an atmosphere of a carbon source and a nitrogen source into the vermiculite-supported iron salt catalyst to react and obtain nitrided carbon nanotubes;

[0147] Specifically: the vermiculite-supported iron salt catalyst is transported to the reactor by inert gas, and the reactor is a two-stage reactor in series; the gas flow rate of the first reactor is 580 L / min of cyclohexane and 600 L / min of inert gas, the reaction temperature is 690°C, and the reaction time is 13 minutes from the entry of cyclohexane to the final discharge; the gas flow rate of the second reactor is 450 L / min of cyclohexane, 100 L / min of ammonia and 580 L / min of inert gas, the reaction temperature is 650°C, and the reaction time is 33 minutes from the entry of the carbon source to the final discharge;

[0148] Pickling treatment:

[0149] 2g of carbon nitride nanotubes and 150ml of n-butanol were mixed and stirred at room temperature for 1 hour, filtered and washed with deionized water for 3 times, 100ml of sulfuric acid and nitric acid solution (sulfuric acid and nitric acid in molar ratio of 1:1, total concentration of 5mol / L) were added to the filtered carbon nanotubes, refluxed and stirred at 90°C for 2h, and finally filtered and washed 5 times, dried in an oven at 60°C, and ground for use;

[0150] S30, using carbon nitride nanotubes to load iridium oxide to obtain an anode catalyst;

[0151] S31, take 1g of iridium oxide, 20g of deionized water and 0.1g of emulsifier OP-10;

[0152] S32, mixing iridium oxide, deionized water and an emulsifier by ultrasonication for 30 minutes, and then using an ultra-high pressure homogenizer for high pressure homogenization to obtain a first mixture, wherein the turbulent pressure is 20 MPa, the time is 40 min, and the slurry volume circulation flow rate is 120 ml / min;

[0153] S33. Then, 1 g of acid-washed carbon nitride nanotubes is added to the first mixture for a second high-pressure homogenization, wherein the turbulent pressure is 10 MPa, the time is 30 min, and the slurry volume circulation flow rate is 50 ml / min; finally, low-temperature ultrasound is applied at 5°C for 30 minutes, and then the mixture is dried in an oven at 60°C and ground for standby use to obtain the anode catalyst.

[0154] Comparative Example 1

[0155] Compared with Example 1, iridium oxide prepared by the preparation method provided in Example 1 is used as the anode catalyst.

[0156] Comparative Example 2

[0157] Compared with Example 1, commercially available nitrogen-doped carbon nanotubes were used to load iridium oxide to obtain an anode catalyst.

[0158] Comparative Example 3

[0159] Commercially available iridium oxide was directly used as the anode catalyst.

[0160] Performance Testing

[0161] Weigh the anode catalyst powder obtained in Examples 1-3 and Comparative Examples 1-3, add a certain proportion of pure water, isopropanol and Nafion solution in turn, mix, ultrasonicate the mixture to make it uniform, and obtain an anode slurry for use. Among them, the mass ratio of each component is as follows: anode catalyst: Nafion = 1:2, isopropanol: pure water = 1:1, iridium oxide catalyst: (mixed solution of isopropanol and pure water) = 1:35. Take 40% Pt / C as the cathode catalyst, repeat the above steps to obtain a cathode slurry for use. Among them, 40% Pt / C is a cathode catalyst with carbon as the catalyst carrier and Pt as the metal-loaded cathode catalyst, and the mass ratio of metal Pt is 40%. The cathode slurry and the anode slurry are respectively loaded into the spraying device and sprayed on both sides of the proton exchange membrane respectively, and the metal iridium loading on the anode surface is 0.3mg / cm 2 , cathode metal platinum loading 0.3mg / cm 2 , dried at 80°C, and placed on a hot press for hot pressing to prepare membrane electrodes.

[0162] (1) The membrane electrode was installed in a water electrolysis test platform, a constant current power supply was applied for trial operation, and the voltage of the membrane electrode having the iridium oxide catalyst at different current densities was tested.

[0163] (2) In order to study the stability of the prepared anode catalyst in an acidic electrochemical environment, each catalyst was subjected to an accelerated durability test (ADT) at 100 mVs -1 The scanning rate is 1.2~1.6vsRHE(0.544~0.944vs Hg 2 SO 4 ) for 3000 cycles. CV and LSV data were collected before and after the cycle according to the above method, and the electrochemical stability of the catalyst was evaluated by comparing the overpotential loss (decay rate %) of the catalyst at different cycles. The test results are shown in the table below: 2 Voltage statistics under current density (performance comparison of different iridium oxide loadings and pure iridium oxide)

[0164] Example Catalyst iridium oxide content <![CDATA[10mA / cm 2 Lower voltage value]]> <![CDATA[Anode iridium loading (mg / cm 2 )]]> Attenuation rate % Example 1 <![CDATA[IrO 2 -26%]]> 1.789 <![CDATA[0.28mg / cm 2 ]]> 2.5% Example 2 <![CDATA[IrO 2 -29%]]> 1.815 <![CDATA[0.32mg / cm 2 ]]> 2.8% Example 3 <![CDATA[IrO 2 -35%]]> 1.848 <![CDATA[0.36mg / cm 2 ]]> 3.3% Comparative Example 1 <![CDATA[Self-made IrO 2 > 1.853 <![CDATA[0.7mg / cm 2 ]]> 0.4% Comparative Example 2 <![CDATA[IrO 2 -13%]]> 1.542 <![CDATA[0.10mg / cm 2 ]]> 5.6% Comparative Example 3 <![CDATA[Commercially available IrO 2 > 1.850 <![CDATA[0.9mg / cm 2 ]]> 0%

[0165] Comparative Example 3 Commercially available IrO 2 It is a rutile phase, so its LSV curves before and after 3000 cycles of CV accelerated cycle test overlap, and after 3000 cycles of CV accelerated durability test, the catalyst decay rate is 0, with excellent durability. The carbon nanotube-loaded iridium oxide anode catalysts prepared in Examples 1 to 3 of the present application, because the stability of carbon nitride nanotubes in an acidic electrochemical environment is not as good as iridium oxide, but the LSV curves before and after 3000 cycles of CV accelerated cycle test are basically overlapped, and the decay rate is only about 3%, the key point is that the activity has been significantly improved. In other words, compared with Comparative Example 3, the carbon nanotube-loaded iridium oxide catalyst prepared in the examples of the present application has significantly improved activity while taking into account excellent durability.

[0166] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0167] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing an anode catalyst for producing hydrogen by electrolysis of water, It is characterized in that include: Providing iridium oxide; preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes; The carbon nitride nanotubes are used to load the iridium oxide to obtain the anode catalyst.

2. The preparation method according to claim 1, It is characterized in that The step of preparing carbon nanotubes and nitrogen-doping the carbon nanotubes to obtain nitrided carbon nanotubes comprises: Providing a layered catalyst with a metal supported on a carrier; The atmosphere of carbon source and nitrogen source is introduced into the layered catalyst to react and obtain nitrided carbon nanotubes.

3. The preparation method according to claim 2, It is characterized in that The step of introducing the atmosphere of the carbon source and the nitrogen source into the layered catalyst to react and obtain the nitrided carbon nanotubes comprises: A first carbon source gas is introduced into the layered catalyst by a fluidized bed process to perform a first catalytic reaction to obtain initial carbon nanotubes attached to the surface of the layered catalyst, and then a second carbon source gas and a nitrogen source gas are introduced to perform a second catalytic reaction to obtain the nitrided carbon nanotubes.

4. The preparation method according to claim 3, It is characterized in that The first carbon source gas and the second carbon source gas include at least one of cyclohexanone and cyclohexane; and / or The nitrogen source gas is ammonia.

5. The preparation method according to claim 1, It is characterized in that The method of using the carbon nitride nanotubes to load the iridium oxide to obtain the anode catalyst comprises: providing a first solvent and an emulsifier; The iridium oxide, the first solvent and the emulsifier are mixed by ultrasound, and then subjected to a first high-pressure homogenization to obtain a first mixture; The carbon nitride nanotubes are added to the first mixture, and a second high-pressure homogenization is performed to obtain the anode catalyst.

6. The preparation method according to claim 5, It is characterized in that After the second high-pressure homogenization, and before obtaining the anode catalyst, ultrasonic treatment, drying and grinding treatment are sequentially performed.

7. The preparation method according to claim 1, It is characterized in that Before the carbon nitride nanotubes are used to load the iridium oxide, the method includes: performing an acid wash treatment on the carbon nitride nanotubes to remove impurities of the carbon nitride nanotubes and introducing functional groups on the surface of the carbon nitride nanotubes to improve the activity and dispersibility of the carbon nitride nanotubes.

8. The preparation method according to claim 7, It is characterized in that The pickling treatment comprises: Dispersing the carbon nitride nanotubes using an organic solvent; Using a first solvent for washing and filtering; A mixed acid solution is used for pickling and post-treatment.

9. The preparation method according to any one of claims 1 to 8, It is characterized in that The iridium oxide is purchased from the market or prepared by the following steps, wherein the preparation of the iridium oxide comprises: Provide chloroiridic acid, ethylene glycol and acid solution; The chloroiridic acid and the ethylene glycol are mixed and reacted under oil bath conditions; After the reaction is completed, an acid solution is added to precipitate iridium; The iridium single substance is heat-treated in an oxygen atmosphere to obtain the iridium oxide.

10. An anode catalyst for use in catalytic water electrolysis to produce hydrogen. It is characterized in that The anode catalyst is prepared by the preparation method according to any one of claims 1 to 9, and the anode catalyst has a mesh-like porous structure.