Composite metal nanosheet and preparation method and application thereof
By doping selenium on tungsten disulfide nanosheets, low-impedance and high-conductivity composite metal nanosheets were prepared, which solved the problem of high power consumption in electrochemical hydrogen evolution reactions, and significantly improved the efficiency and catalytic performance of electrochemical hydrogen evolution. More efficient hydrogen generation is achieved.
Patent Information
- Application Number
- CN202411182897.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, electrochemical hydrogen evolution reaction consumes high power and low catalyst efficiency, resulting in high cost of hydrogen production by electrolysis of water, high environmental pollution, and unsustainable.
The tungsten disulfide nanosheet is produced by hydrothermal reaction between tungsten source, sulfur source and carbon cloth, and heat treatment is carried out in a selenium vapor environment to prepare selenium-doped composite metal nanosheets with low impedance and high conductivity to improve their electrical power Chemical hydrogen evolution catalytic activity.
The charge transfer resistance of the composite metal nanosheets doped after selenium is greatly reduced, and the conductivity and catalytic performance are significantly improved. They can transfer and move electrons more quickly, improve the efficiency of electrochemical hydrogen evolution and reduce electricity consumption.
Smart Images

Figure CN118957668A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrocatalysis, and in particular to a composite metal nanosheet and a preparation method and application thereof. Background Art
[0002] Hydrogen is a carbon-free fuel with the highest energy. After hydrogen is completely burned, it produces water, which means that hydrogen as a fuel will not produce polluting byproducts. It is a green and clean energy with great development prospects. Secondly, hydrogen has a high calorific value. Complete combustion of 1 kg of hydrogen can release 1.43×10 8 J of heat, which is more than three times that of methane and petroleum. Therefore, hydrogen is recognized as an environmentally friendly second renewable energy source and is considered a good substitute for traditional chemical energy. Hydrogen is very common on the earth, but it usually exists in the form of compounds, so the preparation of hydrogen is a great challenge. Therefore, how to produce hydrogen on a large scale and at a low cost in the current industrialization is one of the key research contents of the industry and the key to the widespread application of green energy. Among various hydrogen production technologies, electrochemical hydrogen evolution reaction (HER) has been widely studied due to its simplicity and economic advantages. At present, more than 95% of hydrogen is still produced through chemical hydrogen production processes such as methane steam reforming and water gas, which is costly, environmentally polluting, and uses non-renewable fossil energy as raw materials, which does not meet the strategic needs of future energy development; and the amount of hydrogen produced by water electrolysis only accounts for 4% of the total, and the development prospects are broad, but the electrolysis of water has the problem of high power consumption. The use of high-efficiency catalysts can not only reduce the consumption of electricity, but also improve efficiency.
[0003] Therefore, the development of low-cost and efficient hydrogen evolution catalysts has important economic, environmental and social significance, and can promote clean energy transformation and sustainable development. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing a composite metal nanosheet, wherein the composite metal nanosheet prepared by the method has higher electrochemical hydrogen evolution catalytic activity.
[0005] The second aspect of the present invention also provides a composite metal nanosheet.
[0006] The third aspect of the present invention also provides an application of a composite metal nanosheet.
[0007] According to the first aspect of the present invention, a method for preparing a composite metal nanosheet is provided, comprising the following steps:
[0008] S1, mixing a tungsten source, a sulfur source and a carbon cloth for hydrothermal reaction to obtain an intermediate;
[0009] S2. The intermediate is subjected to heat treatment in an environment of selenium vapor to obtain the product.
[0010] The method for preparing the composite metal nanosheet according to the embodiment of the present invention has at least the following beneficial effects:
[0011] The present invention uses tungsten source and sulfur source as raw materials, grows tungsten disulfide nanosheet intermediates on carbon cloth through hydrothermal reaction, and then heat treats the intermediates in a selenium vapor environment, and the selenium vapor reacts with the tungsten disulfide nanosheet intermediates to obtain selenium-doped composite metal nanosheets. The composite metal nanosheets have low impedance and high conductivity, and have excellent electrocatalytic hydrogen evolution performance.
[0012] Furthermore, after being doped with selenium, the charge transfer resistance of the composite metal nanosheets can be greatly reduced. Selenium doping may reduce the band gap of WS2 nanosheets, so the charge transfer impedance of the composite metal nanosheets can be greatly reduced, which is conducive to the rapid transfer and movement of electrons in the material, indicating that the composite metal nanosheets have better charge transfer ability and stronger conductivity.
[0013] Furthermore, after being doped with selenium, the morphology still shows an interlaced layered nanosheet structure, but most areas form tiny granular protrusions, and the surface of the nanosheet is generally rough. The thin nanosheet structure can provide the material with a richer edge structure, and these tiny particles can add more new catalytic active sites to its surface, which helps to improve the electrochemical hydrogen evolution catalytic performance of the composite metal nanosheet.
[0014] According to some embodiments of the present invention, the temperature of the hydrothermal reaction is 100-300° C. Therefore, within the above temperature range, the prepared sample has complete grain development and small particle size.
[0015] According to some embodiments of the present invention, the hydrothermal reaction time is 10 to 30 hours. Thus, within the above time range, the prepared samples are evenly distributed.
[0016] According to some embodiments of the present invention, the tungsten source is selected from at least one of sodium tungstate, ammonium metatungstate, ammonium tungstate or tungsten hexachloride.
[0017] According to some embodiments of the present invention, the sulfur source is selected from at least one of thiourea, glutathione, thioacetamide, and sodium diethyldithiocarbamate.
[0018] According to some embodiments of the present invention, the molar ratio of the tungsten source to the sulfur source is 1:(2-4).
[0019] According to some embodiments of the present invention, the temperature of the heat treatment is 300-600° C. Therefore, at the temperature of the heat treatment, the selenium powder can be transformed into selenium vapor, which promotes the reaction.
[0020] According to some embodiments of the present invention, the heat treatment time is 0.5 to 3 hours. When the reaction time is less than 0.5 hours, the reaction is incomplete; when the reaction time exceeds 3 hours, the structure of the composite metal nanosheets is affected.
[0021] A composite metal nanosheet provided according to an embodiment of the second aspect of the present invention is prepared by the preparation method described in the first aspect of the present invention.
[0022] Therefore, the composite metal nanosheet of the present invention has low charge transfer impedance and good conductivity; the composite metal nanosheet has good electrochemical hydrogen evolution catalytic performance.
[0023] The third aspect of the present invention provides a composite metal nanosheet as described above; or the use of the composite metal nanosheet prepared by the method for preparing the composite metal nanosheet in electrocatalytic hydrogen production.
[0024] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0026] Figure 1 It is the electron microscope image of the product prepared in Example 1 of the present invention and Comparative Example 1;
[0027] Figure 2 is the XRD diagram of the products prepared in Example 1 and Comparative Example 1 of the present invention;
[0028] Figure 3 It is the EDS spectra of the products prepared in Example 1 and Comparative Example 1 of the present invention;
[0029] Figure 4 1 are polarization curves (a) and Tafel slopes (b) of the products prepared in Example 1 of the present invention and Comparative Example 1;
[0030] Figure 5 It is the electrochemical impedance spectra of the products prepared in Example 1 and Comparative Example 1 of the present invention;
[0031] Figure 6 It is a double-layer capacitance curve diagram of the products prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0032] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0033] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0034] Example 1
[0035] This example provides a composite metal nanosheet, and the preparation method thereof is as follows:
[0036] Carbon cloth pretreatment: cut 2×2.5cm 2 The carbon cloths of different sizes were ultrasonically treated with acetone, anhydrous ethanol and deionized water for 15 min each to clean the dust and impurities on the carbon cloths and to wet them to enhance their hydrophilicity.
[0037] S1. Use an electronic balance to weigh 1.4g Na2WO4·2H2O and 1.12g CH4N2S respectively, dissolve the two materials together in 20mL deionized water, and stir for 30min to make the solution completely dissolved and clear to obtain a precursor solution; transfer the precursor solution into a 50mL polytetrafluoroethylene reactor liner, and vertically place the cleaned carbon cloth into the reactor liner, place the reactor in a forced air drying oven, set the reaction temperature to 250℃, and the reaction time to 24h to obtain a carbon cloth with WS2 nanosheets grown on it.
[0038] S2. Put the carbon cloth with WS2 nanosheets grown on it into a ceramic boat, take another ceramic boat and put 0.1g of selenium powder into it, then put it into a tubular furnace, introduce argon gas, and raise the temperature to 400°C; the selenium powder turns into selenium vapor at the above temperature, and continue to keep warm for 1 hour to obtain composite metal nanosheets (named: WS2 / Se nanosheets).
[0039] Example 2
[0040] This example provides a composite metal nanosheet, and the preparation method thereof is as follows:
[0041] Carbon cloth pretreatment: cut 2×2.5cm 2 The carbon cloths of different sizes were ultrasonically treated with acetone, anhydrous ethanol and deionized water for 15 min each to clean the dust and impurities on the carbon cloths and to wet them to enhance their hydrophilicity.
[0042] S1. Use an electronic balance to weigh 1.4g Na2WO4·2H2O and 1.12g CH4N2S respectively, dissolve the two materials together in 20mL deionized water, and stir for 30min to make the solution completely dissolved and clear to obtain a precursor solution; transfer the precursor solution into a 50mL polytetrafluoroethylene reactor liner, and vertically place the cleaned carbon cloth into the reactor liner, place the reactor in a forced air drying oven, set the reaction temperature to 250℃, and the reaction time to 24h to obtain a carbon cloth with WS2 nanosheets grown on it.
[0043] S2. Place the carbon cloth with WS2 nanosheets grown on it into a ceramic boat, take another ceramic boat and put 0.2 g of selenium powder into it, then place it into a tubular furnace, introduce argon gas, and heat it to 400°C; the selenium powder turns into selenium vapor at the above temperature, and continue to keep warm for 1 hour to obtain composite metal nanosheets.
[0044] Example 3
[0045] This example provides a composite metal nanosheet, and the preparation method thereof is as follows:
[0046] Carbon cloth pretreatment: cut 2×2.5cm 2 The carbon cloths of different sizes were ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 15 min to clean the dust and impurities on the carbon cloths and to wet them to enhance their hydrophilicity.
[0047] S1. Use an electronic balance to weigh 1.4g Na2WO4·2H2O and 1.12g CH4N2S respectively, dissolve the two materials together in 20mL deionized water, and stir for 30min to make the solution completely dissolved and clear to obtain a precursor solution; transfer the precursor solution into a 50mL polytetrafluoroethylene reactor liner, and vertically place the cleaned carbon cloth into the reactor liner at the same time, place the reactor in a forced air drying oven and set the reaction temperature to 250℃ and the reaction time to 24h to obtain a carbon cloth with WS2 nanosheets grown on it.
[0048] S2. Place the carbon cloth with WS2 nanosheets grown on it into a ceramic boat, take another ceramic boat and put 0.5 g of selenium powder into it, then place it into a tubular furnace, introduce argon gas, and heat it to 400°C; the selenium powder turns into selenium vapor at the above temperature, and continue to keep warm for 1 hour to obtain composite metal nanosheets.
[0049] Example 4
[0050] This example provides a composite metal nanosheet, and its preparation method is basically the same as that of Example 3, except that the heat treatment temperature in step S2 is 300°C.
[0051] Example 5
[0052] This example provides a composite metal nanosheet, and its preparation method is basically the same as that of Example 3, except that the heat treatment temperature in step S2 is 600°C.
[0053] Example 6
[0054] This example provides a composite metal nanosheet, and its preparation method is basically the same as that of Example 3, except that the heat treatment time in step S2 is 0.5 h.
[0055] Example 7
[0056] This example provides a composite metal nanosheet, and its preparation method is basically the same as that of Example 3, except that the heat treatment time in step S2 is 3 hours.
[0057] Comparative Example 1
[0058] Comparative Example 1 provides a tungsten disulfide nanosheet, and the preparation method thereof is as follows:
[0059] Carbon cloth pretreatment: cut 2×2.5cm 2 The carbon cloths of different sizes were ultrasonically treated with acetone, anhydrous ethanol and deionized water for 15 min each to clean the dust and impurities on the carbon cloths and to wet them to enhance their hydrophilicity.
[0060] S1. Use an electronic balance to weigh 1.4g Na2WO4·2H2O and 1.12g CH4N2S respectively, dissolve the two materials together in 20mL deionized water, and stir for 30min to make the solution completely dissolved and clear to obtain a precursor solution; transfer the precursor solution into a 50mL polytetrafluoroethylene reactor liner, and vertically place the cleaned carbon cloth into the reactor liner, place the reactor in a forced air drying oven, set the reaction temperature to 250°C, and the reaction time to 24h to obtain a composite metal nanosheet.
[0061] Performance Testing
[0062] SEM Testing
[0063] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were subjected to SEM tests at different magnifications. The results are as follows: Figure 1 As shown, Figure 1 a, 1b and 1c are scanning electron microscope images of tungsten disulfide nanosheets of Comparative Example 1 at different magnifications; Figure 1 d, 1e and 1f are scanning electron microscope images of the composite metal nanosheets prepared in Example 1 at different magnifications. Figure 1a~1c are SEM images of WS2 materials at different magnifications, proving that WS2 materials have been successfully grown on the surface of carbon cloth, and the material presents an interlaced layered nanosheet structure, with tiny granular protrusions formed in a small number of areas, and the surface of the nanosheet is generally smooth. Figure 1 d~1f are SEM images of WS2 / Se materials at different magnifications. After heat treatment, the morphology of the material has not changed much, and the morphology still shows an interlaced layered nanosheet structure, but most areas have formed tiny granular protrusions, and the surface of the nanosheet is generally rough. The thin nanosheet structure can provide the material with a richer edge structure, and this tiny particle can add more new catalytic active sites to its surface, which helps to improve the catalytic performance of WS2 / Se nanosheets.
[0064] XRD test
[0065] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were subjected to XRD testing, and the results are as follows: Figure 2 As shown in the figure, the XRD patterns of WS2 nanosheets and WS2 / Se nanosheets have not changed substantially, and the characteristic diffraction peaks are basically similar. The diffraction peaks in the figure are in good agreement with the peak positions and diffraction intensities of the WS2 standard card (PDF#08-0237). The peak at 25.5° is the diffraction peak of the carbon cloth, and the strong diffraction peaks at 14.4°, 33.5° and 43.9° correspond to the (002), (101) and (105) crystal planes of the standard hexagonal phase WS2 material, respectively. It is worth noting that the diffraction peak position corresponding to the (002) crystal plane of WS2 / Se nanosheets is shifted to the low angle direction by about 0.1° relative to that of WS2 nanosheets, because the atomic radius of Se is larger than that of S, and the heat treatment increases the interplanar spacing of the material, resulting in the diffraction peak position shifting to a low angle.
[0066] EDS spectrum test
[0067] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were subjected to EDS spectrum testing, and the results are as follows: Figure 3 As shown, Figure 3 ad is the EDS spectrum of WS2 material on carbon cloth, where C element comes from the carbon cloth substrate, and W and S elements come from WS2 nanosheets, indicating that the synthesized WS2 material does not contain other impurities. The distribution of W and S elements matches the shape of the selected scanning area very well, indicating that WS2 material grows well on the carbon cloth and grows relatively uniformly. Figure 3ei is the EDS energy spectrum of WS2 / Se material on carbon cloth. It can be seen from the figure that WS2 / Se nanosheets on carbon cloth contain four elements: C, W, S, and Se, and the distribution is relatively uniform, indicating that the Se element is successfully doped into the WS2 nanosheets, and no other impurities are introduced during the Se doping process.
[0068] Electrochemical performance test
[0069] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were subjected to polarization curve and Tafel slope tests, and the experimental method was as follows:
[0070] A standard three-electrode system was used to test the electrochemical hydrogen evolution catalytic performance of WS2 nanosheets and WS2 / Se nanosheets. The WS2 nanosheets and WS2 / Se nanosheets grown on carbon cloth were directly used as working electrodes with an effective area of approximately 0.5 cm 2 Carbon rod and silver-silver chloride (Ag / AgCl) electrode were selected as counter electrode and reference electrode respectively, and H2SO4 electrolyte with a concentration of 0.5 mol / L was used. The Tafel slope was obtained from the polarization curve.
[0071] Linear sweep voltammetry (LSV) tests were performed on WS2 nanosheets, WS2 / Se nanosheets and platinum carbon (Pt / C) electrodes, with the scan rate set at 5 mV / s. Figure 4 a is the LSV curve of WS2 nanosheets, WS2 / Se nanosheets and Pt / C electrode. It can be seen from the figure that WS2 / Se nanosheets show excellent electrochemical hydrogen evolution catalytic activity. 2 The overpotential of WS2 / Se nanosheets was 215 mV. For comparison, WS2 nanosheets were tested using the same method and conditions. The results showed that the catalytic performance of WS2 nanosheets was relatively poor. 2 When the overpotential of WS2 nanosheets is 287 mV, it indicates that its catalytic effect is significantly worse than that of WS2 / Se nanosheets. The Pt / C electrode exhibits the best catalytic performance, and its overpotential is the smallest at the same current density.
[0072] Figure 4b is the Tafel slope curve of WS2 nanosheet, WS2 / Se nanosheet and Pt / C electrode. As can be seen from the figure, the Tafel slope of WS2 / Se nanosheet in Example 1 of the present invention is 63.01mV / dec, while the Tafel slope of WS2 nanosheet is 108.41mV / dec, and the Tafel slope of Pt / C electrode is 40.56mV / dec. The Tafel slope value of WS2 / Se nanosheet is much smaller than that of WS2 nanosheet, and the difference of Tafel slope from Pt / C is also greatly reduced, showing better catalytic performance.
[0073] Impedance test
[0074] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were subjected to EIS test, and the results are as follows: Figure 5 As shown, the charge transfer resistance (R ct ) has a smaller value of about 52.71Ω, and the charge transfer resistance of the composite metal nanosheets after Se doping can still be greatly reduced. The charge transfer resistance (R ct ) is only 15.47Ω. The doping of Se element may reduce the band gap of WS2 nanosheets, so the charge transfer impedance of WS2 / Se nanosheets can be greatly reduced, which is conducive to the rapid transfer and movement of electrons in the material, indicating that WS2 / Se nanosheets have better charge transfer ability and stronger conductivity, which further indicates that they have better electrochemical hydrogen evolution catalytic activity.
[0075] Double layer capacitance curve experiment
[0076] The composite metal nanosheets prepared in Example 1 of the present invention and the tungsten disulfide nanosheets prepared in Comparative Example 1 were tested for double-layer capacitance curves. The results are as follows: Figure 6 As shown, the C of the composite metal nanosheets dl The value is 43.44mF / cm 2 , while the C of WS2 nanosheets dl The value is 29.71mF / cm 2 By comparison, it can be found that the ECSA of WS2 / Se nanosheets is 1.4 times that of WS2 nanosheets. It is precisely because WS2 / Se has a larger ECSA that it has better electrochemical hydrogen evolution catalytic activity.
[0077] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A method for preparing a composite metal nanosheet, characterized in that: The method comprises the following steps: S1, mixing a tungsten source, a sulfur source and a carbon cloth for hydrothermal reaction to obtain an intermediate; S2. The intermediate is subjected to heat treatment in an environment of selenium vapor to obtain the product.
2. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 100-300°C.
3. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The hydrothermal reaction time is 10 to 30 hours.
4. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The tungsten source is selected from at least one of sodium tungstate, ammonium metatungstate, ammonium tungstate oxide or tungsten hexachloride.
5. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The sulfur source is selected from at least one of thiourea, glutathione, thioacetamide, and sodium diethyldithiocarbamate.
6. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The molar ratio of the tungsten source to the sulfur source is 1:(2-4).
7. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The temperature of the heat treatment is 300-600°C.
8. The method for preparing the composite metal nanosheet according to claim 1, characterized in that: The heat treatment time is 0.5 to 3 hours.
9. A composite metal nanosheet, characterized in that: The method is prepared by the method according to any one of claims 1 to 8.
10. Use of the composite metal nanosheet according to claim 9; or the composite metal nanosheet prepared by the method for preparing the composite metal nanosheet according to any one of claims 1 to 8 in electrocatalytic hydrogen production.