Solid solution alloy negative electrode material and preparation method and application thereof

By constructing a solid solution alloy negative electrode material on the surface of zinc sheets of zinc air batteries, the problem of poor electrochemical reversibility caused by zinc dendrites in zinc air batteries is solved, which extends the battery life and improves the circulation performance and power density.

CN118957684APending Publication Date: 2024-11-15NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410858516.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In alkaline electrolyte, zinc-air batteries have poor electrochemical reversibility due to the dendrite problem of zinc metal negative electrode, which reduces the working life of zinc-air batteries.

Method used

Using the preparation method of solid solution alloy negative electrode material, the carbon nanotubes and thiourea are acidified to form NC material, and then mixed with red phosphorus, added conductive agent and binder, coated on the surface of zinc sheet, and passed through electricity Deposition forms P-NC material, and an artificial protective layer is constructed to regulate zinc ion flux and inhibit dendrites' growth.

Benefits of technology

It effectively extends the service life of zinc air batteries, reduces the formation of zinc dendrites and battery short circuit problems, achieves uniform deposition of zinc ions and electrolyte ions to more easily contact the zinc anode, and improves the cycling performance and power density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957684A_ABST
    Figure CN118957684A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of zinc air batteries, in particular to a solid solution alloy negative electrode material and a preparation method and application thereof. The preparation method of the solid solution alloy negative electrode material comprises the following steps: adding acidified carbon nanotubes and thiourea into water, stirring, removing moisture, and sintering in an inert atmosphere to obtain an NC material; mixing the NC material with red phosphorus, and carrying out heat preservation at 470-550 DEG C in an inert atmosphere to obtain a P-NC material; mixing the P-NC material with a conductive agent, a binder and a solvent to prepare slurry, coating the surface of a zinc sheet with the slurry, and drying to prepare a zinc electrode; a zinc electrode is used as a working electrode, an Ag / AgCl electrode is used as a reference electrode, a carbon rod is used as a counter electrode, the three-system electrode is subjected to electro-deposition in electro-deposition liquid, and the electrode is obtained. The electro-deposition liquid contains zinc ions. The protective layer is constructed on the surface of the zinc anode, so that the zinc anode is effectively protected from being corroded by alkaline electrolyte, and the growth of dendritic crystals in the circulation process is inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of zinc-air batteries, and in particular to a solid solution alloy negative electrode material and a preparation method and application thereof. Background Art

[0002] In the field of new energy, batteries are a widely used energy storage technology. Especially in recent years, society has paid more and more attention to new energy technologies, and various battery technologies have developed rapidly. Among them, air batteries have the advantages of being green and pollution-free, high energy conversion efficiency, fast start-up speed, long service life and dry storage time, and have broad application potential in the field of new energy.

[0003] However, there are still some problems with air batteries. The oxygen reduction reaction kinetics of their electrodes are slow, and their costs are high and reserves are low, which greatly restricts the large-scale application of air batteries.

[0004] The invention patent application with application publication number CN110112427A discloses a method for preparing an electrochemically assisted nitrogen and phosphorus dual-doped carbon-based air electrode, the method comprising: (1) pretreatment of a conductive carbon substrate: washing the conductive carbon substrate with an organic solvent such as acetone, anhydrous ethanol and deionized water, then immersing the conductive carbon substrate in a mixed acid of sulfuric acid and nitric acid, and completely drying after the treatment; (2) preparation of a polymerization electrolyte, selecting an organic ligand containing a nitrogen element and a compound containing a phosphorus element that can be electrochemically polymerized as reactants, dissolving the above reactants in a solvent, Prepare a polymer electrolyte, or further include an electrolyte soluble in the solvent in the above polymer electrolyte; (3) Preparation of nitrogen and phosphorus dual-doped carbon-based air electrode, using the conductive carbon substrate of step (1) as the working electrode, the above-mentioned polymer electrolyte as the electrolyte, using a three-electrode system, polymerizing on the conductive carbon substrate to generate a polymer containing nitrogen and phosphorus, drying the reacted conductive carbon substrate, placing the conductive carbon substrate coated with the polymer in an inert gas, setting a heating program, and performing high-temperature calcination to finally obtain a nitrogen and phosphorus dual-doped carbon-based air electrode.

[0005] The material prepared by this method has good catalytic performance and can improve the reaction efficiency. However, it uses carbon materials such as carbon cloth as the matrix, and the electrochemical performance is poor. For zinc-air batteries, using zinc as the negative electrode has a larger capacity, which can reach 5850Ah·L-1, and a high electrochemical reduction potential (-0.76V vs SHE). In addition, the zinc negative electrode is highly compatible with aqueous electrolytes, which provides favorable conditions for the large-scale promotion of zinc-air batteries. However, many problems have been found in the application of rechargeable secondary zinc-air batteries in many fields. For example, in alkaline electrolytes, the electrochemical reversibility of the zinc metal negative electrode is poor due to problems such as dendrites, which reduces the working life of the zinc-air battery. Summary of the invention

[0006] In order to improve the cycle performance of zinc-air batteries, one of the purposes of the present invention is to provide a method for preparing a solid solution alloy negative electrode material.

[0007] The second object of the present invention is to provide a solid solution alloy negative electrode material prepared by the above preparation method.

[0008] The third object of the present invention is to provide the application of the above-mentioned solid solution alloy negative electrode material.

[0009] To achieve the above object, the technical solution adopted by the present invention is:

[0010] A method for preparing a solid solution alloy negative electrode material comprises the following steps:

[0011] 1) acidifying the carbon nanotubes, then adding the acidified carbon nanotubes and thiourea into water, stirring for 1-2 hours, and removing water by rotary evaporation to obtain a precursor;

[0012] 2) The precursor prepared in step 1) is kept at 700-800° C. for 3-5 hours in an inert atmosphere to obtain an NC material;

[0013] 3) mixing the NC material obtained in step 2) with red phosphorus, keeping the mixture at 470-550° C. for 3-6 hours under an inert atmosphere, then cooling the mixture to 230-280° C. for 1-3 hours to obtain a P-NC material;

[0014] 4) mixing the P-NC material obtained in step 3) with a conductive agent, a binder, and a solvent to prepare a slurry, and then coating the slurry on the surface of the zinc sheet and drying the slurry to obtain a zinc electrode;

[0015] 5) Using the zinc electrode prepared in step 4) as the working electrode, the Ag / AgCl electrode as the reference electrode, and the carbon rod as the counter electrode, the three-system electrode is subjected to electrodeposition in an electrodeposition solution to obtain; the electrodeposition solution contains zinc ions.

[0016] The solid solution alloy negative electrode material prepared by the above method is on the surface of the zinc sheet. If necessary, the material can be peeled off from the surface of the zinc sheet. The peeling method can adopt the method in the prior art. Of course, if the zinc sheet with the material is directly used, peeling is not required.

[0017] In step 1), the acidification treatment is carried out by soaking in a mixed solution of concentrated nitric acid and concentrated sulfuric acid. The volume ratio of concentrated nitric acid to concentrated sulfuric acid is 1:1.

[0018] The mass ratio of carbon nanotubes to thiourea in step 1) is 0.02-0.03:0.5-2. The amount of water used in step 1) is 100-200 mL of water for every 0.5-2 g of thiourea.

[0019] In step 2), the temperature is kept at 700-800℃ for 2℃·min. -1 The temperature is raised to 700-800°C at a heating rate and then kept warm.

[0020] In step 2), the inert atmosphere is argon.

[0021] In step 2), after being kept at 700-800° C. for 3-5 hours, the temperature is lowered, and the mixture is washed with water and ethanol in sequence, and dried in a vacuum oven at 60-80° C. overnight to obtain the NC material.

[0022] In step 3), the mass ratio of NC material to red phosphorus is 3-5:1.

[0023] In step 3), the temperature is kept at 470-550℃ for 3-6h, and the temperature is firstly increased at 2℃·min -1 The temperature is raised to 470-550°C at a heating rate and then kept at this temperature for 3-6 hours.

[0024] The cooling rate in step 3) to 230-280°C is 1°C min -1 .

[0025] In step 4), the mass ratio of the P-NC material to the conductive agent and the binder is 65-85:12-18:5-15. The conductive agent is at least one of carbon black and graphene. The binder is polyvinylidene fluoride. The solvent is at least one of nitrogen methyl pyrrolidone and polyvinyl pyrrolidone.

[0026] In step 4), the mass fraction of the binder in the slurry is 1%-3%.

[0027] In step 4), the drying is carried out in a vacuum oven at 60-80° C. for 10-15 hours.

[0028] In step 4), the zinc sheet is pretreated before use, and the pretreatment includes: grinding the zinc sheet with sandpaper of different mesh sizes, the mesh size of the sandpaper used each time is increased successively, then putting it into water, using ultrasound treatment, then taking it out, washing it with anhydrous ethanol for multiple times, and drying it at room temperature. Preferably, the mesh sizes of the sandpaper used are 500 mesh, 600 mesh, 800 mesh, and 1000 mesh, respectively.

[0029] The electrodeposition in step 5) is constant current electrodeposition.

[0030] In step 5), the electrodeposition solution is prepared by dissolving a soluble zinc salt, boric acid, a soluble sodium salt, and disodium ethylenediaminetetraacetate in water. The soluble zinc salt is at least one of zinc sulfate, zinc chloride, and zinc nitrate. The soluble sodium salt is at least one of sodium sulfate, sodium chloride, and sodium nitrate. Further, the soluble sodium salt is at least two of sodium sulfate, sodium chloride, and sodium nitrate. Further, the electrodeposition solution is prepared by dissolving zinc sulfate, boric acid, sodium sulfate, sodium chloride, and disodium ethylenediaminetetraacetate in water.

[0031] The concentration of the soluble zinc salt in the electrodeposition solution is 0.3-0.5 mol / L.

[0032] The concentration of boric acid in the electrodeposition solution is 0.06-0.09 mol / L.

[0033] The concentration of soluble sodium salt in the electrodeposition solution is 0.5-0.8 mol / L.

[0034] The soluble sodium salt is composed of sodium sulfate and sodium chloride. The concentration of sodium sulfate in the electrodeposition solution is 0.2-0.3 mol / L. The concentration of sodium chloride in the electrodeposition solution is 0.3-0.5 mol / L.

[0035] The concentration of disodium ethylenediaminetetraacetate in the electrodeposition solution is 0.005-0.008 mol / L.

[0036] The voltage of the electrodeposition in step 5) is 0.8-2V, preferably 1V-1.8V.

[0037] In step 5), the current of the electrodeposition is 20-60 mA and the electrodeposition time is 30-300 s.

[0038] A solid solution alloy negative electrode material prepared by the above method.

[0039] Application of the above-mentioned solid solution alloy negative electrode material in zinc-air batteries.

[0040] The zinc-air battery comprises

[0041] The comprehensive beneficial effects of the present invention are:

[0042] The present invention modifies the surface of zinc sheet (zinc foil), and the N-doped carbon framework has good conductivity, which can adjust the uniform distribution of the electric field on the electrode surface. The high nucleation overpotential of the P-doped P-NC reduces the deposition kinetics of zinc ions, which has a positive effect on the refinement of particles and uniform precipitation. Compared with the traditional Zn electrode, the hydrophobicity of the ZnP-NC coating prepared in the present application makes it easier for electrolyte ions to contact the zinc anode, which is conducive to adjusting the zinc ion flux, achieving uniform deposition on the anode surface, reducing the formation of zinc dendrites and the problem of piercing the diaphragm to cause battery short circuit, and extending the service life of the battery.

[0043] The present application constructs an artificial protective layer on the surface of the zinc negative electrode (anode), which has a dual role: effectively protecting the zinc anode from corrosion by alkaline electrolytes and inhibiting the growth of dendrites and hydrogen evolution during the cycle. The material layer structure on the surface of the zinc negative electrode can reshape the zinc ion flux near the interface, allowing zinc ions to diffuse evenly on the surface of the zinc electrode, achieving uniform zinc deposition, and inhibiting the uncontrolled growth of zinc dendrites. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a scanning electron microscope (SEM) image of the Zn@ZnP-NC solid solution alloy anode prepared in Example 1 of the present invention;

[0045] Figure 2 This is a scanning electron microscope (SEM) image of the Zn@ZnP-NC solid solution alloy anode prepared in Example 1 of the present invention after long-term cycling;

[0046] Figure 3 A comparison chart of symmetrical battery cycle performances obtained by using the Zn@ZnP-NC solid solution alloy anode prepared in Example 1 of the present invention and the Zn anode of Comparative Example 1;

[0047] Figure 4 Full cell power density curves obtained for the Zn@ZnP-NC solid solution alloy anode prepared in Example 1 of the present invention and the Zn anode of Comparative Example 1;

[0048] Figure 5 This is a comparison chart of the full battery cycle performance of the Zn@ZnP-NC solid solution alloy anode prepared in Example 1 of the present invention and the Zn anode of Comparative Example 1. DETAILED DESCRIPTION

[0049] In order to make the technical problems solved by the present invention, the technical solutions adopted and the technical effects achieved easier to understand, the technical solutions of the present invention are clearly and completely described below in conjunction with specific embodiments.

[0050] Example 1

[0051] The preparation method of the solid solution alloy negative electrode material of this embodiment comprises the following steps:

[0052] 1) Cut the zinc sheet into a size of 2.5 cm × 1 cm, and polish it with sandpaper of 500 mesh, 600 mesh, 800 mesh, and 1000 mesh in sequence. Then, ultrasonically treat the zinc sheet in pure water for 3 min, rinse it with anhydrous ethanol 5 times, and dry it at room temperature;

[0053] 2) adding 0.025 g of carbon nanotubes to a mixed solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1, soaking, then adding the soaked carbon nanotubes and 1 g of thiourea (CH4N2S) to 150 ml of deionized water, stirring for 1 hour; removing water by rotary evaporation, and collecting the precursor material;

[0054] 3) The precursor material collected in step 2) was heated at 2°C·min in an argon (Ar) atmosphere. -1 The temperature was raised to 750°C at a rate of 1.5 ℃, kept at this temperature for 4 h in an argon (Ar) atmosphere, cooled, washed with deionized water and ethanol, and dried in a vacuum oven at 70°C overnight to obtain NC material;

[0055] 4) The NC material obtained in step 3) was mixed with red phosphorus at a mass ratio of 4:1, sealed in a quartz tube, and heated at 2°C min in an argon atmosphere of the quartz tube. -1 The temperature was raised to 500°C at a rate of 1°C / min, kept at that temperature for 4 h, and then cooled to 260°C and kept at that temperature for 2 h. The cooling rate was 1°C / min -1 , and then cooled to room temperature to obtain the P-NC material.

[0056] 5) adding P-NC material, carbon black conductive agent and polyvinylidene fluoride (PVDF) in a mass ratio of 75:15:10 to N-methylpyrrolidone (NMP), mixing evenly to obtain a slurry, wherein the mass fraction of PVDF is 1.5%; coating the slurry on the surface of the zinc sheet treated in step 1), placing it in a vacuum oven at 70° C. and drying it for 12 hours to obtain a zinc electrode;

[0057] 6) Zinc sulfate heptahydrate (ZnSO4·7H2O), boric acid (H3BO3), sodium sulfate (Na2SO4), sodium chloride (NaCl), disodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8) was dissolved in 50ml of deionized water to prepare an electrodeposition solution; the concentrations of zinc sulfate, boric acid, sodium sulfate, sodium chloride, and disodium ethylenediaminetetraacetate in the electrodeposition solution were 0.4mol / L, 0.08mol / L, 0.28mol / L, 0.34mol / L, and 0.006mol / L, respectively;

[0058] The zinc electrode obtained in step 5) is used as the working electrode, the Ag / AgCl electrode is selected as the reference electrode, and the carbon rod is selected as the counter electrode. The three-electrode system is immersed in the above-mentioned electrodeposition solution, the voltage is controlled at about 1V to 1.8V, the current size is set to -50mA, and the electrodeposition is carried out for 60s in a laboratory environment. After the electrodeposition is completed, the electrode surface is cleaned with deionized water for many times and dried at room temperature to obtain a solid solution alloy negative electrode. The material on the surface of the zinc sheet is scraped off to obtain a solid solution alloy negative electrode material.

[0059] Example 2

[0060] The preparation method of the solid solution alloy negative electrode material of this embodiment comprises the following steps:

[0061] 1) Cut the zinc sheet into a size of 2.5 cm × 1 cm, and polish it with sandpaper of 500 mesh, 600 mesh, 800 mesh, and 1000 mesh in sequence. Then, ultrasonically treat the zinc sheet in pure water for 3 min, rinse it with anhydrous ethanol 5 times, and dry it at room temperature;

[0062] 2) adding 0.03 g of carbon nanotubes to a mixed solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1, soaking, then adding the soaked carbon nanotubes and 1 g of thiourea (CH4N2S) to 150 ml of deionized water, stirring for 1 hour; removing water by rotary evaporation, and collecting the mixture;

[0063] 3) The mixture collected in step 2) was heated at 2°C·min under argon (Ar) atmosphere. -1 The temperature was raised to 780°C at a rate of 1.5 ℃, kept at this temperature for 3 h in an argon (Ar) atmosphere, cooled, washed with deionized water and ethanol, and dried in a vacuum oven at 70°C overnight to obtain NC material;

[0064] 4) The NC material obtained in step 3) was mixed with red phosphorus at a mass ratio of 4.25:1, sealed in a quartz tube, and heated at 2°C min in an argon atmosphere of the quartz tube. -1 The temperature was raised to 550°C at a rate of 1°C / min and kept at that temperature for 3 h. The temperature was then lowered to 250°C and kept at that temperature for 2 h. The cooling rate was 1°C / min. -1 , and then cooled to room temperature to obtain the P-NC material.

[0065] 5) adding P-NC material, carbon black conductive agent and polyvinylidene fluoride (PVDF) in a mass ratio of 75:15:10 to N-methylpyrrolidone (NMP), mixing evenly to obtain a slurry, wherein the mass fraction of PVDF is 1.5%; coating the slurry on the surface of the zinc sheet treated in step 1), placing it in a vacuum oven at 70° C. and drying it for 12 hours to obtain a zinc electrode;

[0066] 6) Zinc sulfate heptahydrate (ZnSO4·7H2O), boric acid (H3BO3), sodium sulfate (Na2SO4), sodium chloride (NaCl), disodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8) was dissolved in 50ml of deionized water to prepare an electrodeposition solution; the concentrations of zinc sulfate, boric acid, sodium sulfate, sodium chloride, and disodium ethylenediaminetetraacetate in the electrodeposition solution were 0.5mol / L, 0.09mol / L, 0.3mol / L, 0.45mol / L, and 0.005mol / L, respectively;

[0067] The zinc electrode obtained in step 5) is used as the working electrode, the Ag / AgCl electrode is selected as the reference electrode, and the carbon rod is selected as the counter electrode. The three-electrode system is immersed in the above-mentioned electrodeposition solution, the voltage is controlled at about 1V to 1.8V, the current size is set to -50mA, and the electrodeposition is carried out for 60s in a laboratory environment. After the electrodeposition is completed, the electrode surface is cleaned with deionized water for many times and dried at room temperature to obtain a solid solution alloy negative electrode. The material on the surface of the zinc sheet is scraped off to obtain a solid solution alloy negative electrode material.

[0068] Example 3

[0069] The preparation method of the solid solution alloy negative electrode material of this embodiment comprises the following steps:

[0070] 1) Cut the zinc sheet into a size of 2.5 cm × 1 cm, and polish it with sandpaper of 500 mesh, 600 mesh, 800 mesh, and 1000 mesh in sequence. Then, ultrasonically treat the zinc sheet in pure water for 3 min, rinse it with anhydrous ethanol 5 times, and dry it at room temperature;

[0071] 2) adding 0.02 g of carbon nanotubes to a mixed solution of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1, soaking, then adding the soaked carbon nanotubes and 1 g of thiourea (CH4N2S) to 150 ml of deionized water, stirring for 1 hour; removing water by rotary evaporation, and collecting the mixture;

[0072] 3) The mixture collected in step 2) was heated at 2°C·min under argon (Ar) atmosphere. -1 The temperature was raised to 725°C at a rate of 1.5 ℃, kept at this temperature for 5 h in an argon (Ar) atmosphere, cooled, washed with deionized water and ethanol, and dried in a vacuum oven at 60°C overnight to obtain NC material;

[0073] 4) The NC material obtained in step 3) was mixed with red phosphorus at a mass ratio of 3.5:1, sealed in a quartz tube, and heated at 2°C min in an argon atmosphere of the quartz tube. -1 The temperature was raised to 470℃ at a rate of 1℃·min, kept at that temperature for 5h, then cooled to 270℃, kept at that temperature for 2h, and the cooling rate was 1℃·min -1 , and then cooled to room temperature to obtain the P-NC material.

[0074] 5) adding P-NC material, carbon black conductive agent and polyvinylidene fluoride (PVDF) in a mass ratio of 75:15:10 to N-methylpyrrolidone (NMP), mixing evenly to obtain a slurry, wherein the mass fraction of PVDF is 1.5%; coating the slurry on the surface of the zinc sheet treated in step 1), placing it in a vacuum oven at 70° C. and drying it for 12 hours to obtain a zinc electrode;

[0075] 6) Zinc sulfate heptahydrate (ZnSO4·7H2O), boric acid (H3BO3), sodium sulfate (Na2SO4), sodium chloride (NaCl), disodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8) was dissolved in 50mL of deionized water to prepare an electrodeposition solution; the concentrations of zinc sulfate, boric acid, sodium sulfate, sodium chloride, and disodium ethylenediaminetetraacetate in the electrodeposition solution were 0.35mol / L, 0.06mol / L, 0.25mol / L, 0.3mol / L, and 0.008mol / L, respectively;

[0076] The zinc electrode obtained in step 5) is used as the working electrode, the Ag / AgCl electrode is selected as the reference electrode, and the carbon rod is selected as the counter electrode. The three-electrode system is immersed in the above-mentioned electrodeposition solution, the voltage is controlled at about 1V-1.8V, the current size is set to -50mA, and the electrodeposition is carried out for 60s under a laboratory environment. After the electrodeposition is completed, the electrode surface is cleaned with deionized water for multiple times and dried at room temperature to obtain a solid solution alloy negative electrode. The material on the surface of the zinc sheet is scraped off to obtain a solid solution alloy negative electrode material.

[0077] Comparative Example 1

[0078] The preparation method of the alloy negative electrode material of the comparative example comprises the following steps:

[0079] 1) Cut the zinc sheet into 2.5 cm × 1 cm specifications, and polish it with sandpaper of 500 mesh, 600 mesh, 800 mesh, and 1000 mesh. Then put the zinc sheet in pure water, treat it with ultrasound for 3 minutes, rinse it with anhydrous ethanol 5 times, and dry it at room temperature;

[0080] 2) Zinc sulfate heptahydrate (ZnSO4·7H2O), boric acid (H3BO3), sodium sulfate (Na2SO4), sodium chloride (NaCl), disodium ethylenediaminetetraacetate (C 10 H 14 N2Na2O8) was dissolved in 50ml of deionized water to prepare an electrodeposition solution; the concentrations of zinc sulfate, boric acid, sodium sulfate, sodium chloride, and disodium ethylenediaminetetraacetate in the electrodeposition solution were 0.4mol / L, 0.08mol / L, 0.28mol / L, 0.34mol / L, and 0.006mol / L, respectively;

[0081] 3) The zinc sheet treated in step 1) is used as the working electrode, the Ag / AgCl electrode is selected as the reference electrode, and the carbon rod is selected as the counter electrode. The three-electrode system is immersed in the electrodeposition solution prepared in step 2), the voltage is controlled at about 1V-1.8V, the current is set to -50mA, and electroplating is performed for 60s in a laboratory environment. After the electroplating is completed, the electrode surface is cleaned with deionized water several times and dried at room temperature to obtain an alloy negative electrode. The material on the surface of the zinc sheet is scraped off to obtain an alloy negative electrode material.

[0082] Test example

[0083] (1) Morphology test

[0084] The solid solution zinc alloy negative electrode material prepared in Example 1 was scraped off the zinc sheet and subjected to SEM testing. The results are as follows: Figure 1 shown.

[0085] from Figure 1 It can be seen that the microstructure of the solid solution alloy zinc negative electrode material Zn@ZnP-NC is a cluster structure similar to petals.

[0086] (2) Electrochemical test

[0087] The alloy zinc negative electrode (zinc sheet with alloy zinc negative electrode material) prepared in Example 1 and the comparative example was used as the negative electrode and assembled with carbon cloth loaded with Pt / C and RuO2 in an acrylic zinc-air battery mold. A hydrophobic film was attached to the electrolyte layer-air layer interface, and 6 mol / L KOH and 0.2 mol / L Zn(CH3COO)2 solution were injected to obtain an alkaline zinc-air battery.

[0088] The battery was cycle tested for 200 hours using the Xinwei system.

[0089] The electrode after cycling was taken out, the solid solution alloy zinc negative electrode material on the surface of the zinc sheet was scraped off, and SEM test was performed. The test results are as follows Figure 2 shown.

[0090] from Figure 2 It can be seen that after a long period of cycling, no zinc dendrites appear on the surface of the negative electrode material. (Dendrites should form on the electrode surface)

[0091] After the zinc-air battery prepared with the alloy zinc negative electrode of Example 1 and Comparative Example 1 was charged and discharged, its charge and discharge power density was calculated, as shown in FIG. Figure 3 shown.

[0092] Depend on Figure 3 It can be seen that the zinc-air battery made with the alloy zinc negative electrode of Example 1 has a higher power density.

[0093] The alloy zinc negative electrodes prepared in Example 1 and the comparative example were used to prepare symmetrical batteries, and the charge and discharge cycles were performed. The results are as follows: Figure 4 shown.

[0094] from Figure 4 It can be seen that the battery corresponding to Example 1 has better cycle stability.

[0095] The alloy zinc negative electrodes prepared in Example 1 and the comparative example were used to prepare full batteries and the charge and discharge cycles were performed. The results are as follows: Figure 5 shown.

[0096] from Figure 5 It can be seen that the battery corresponding to Example 1 has a longer cycle time and better cycle performance.

[0097] The above description is only preferred embodiments and test examples of the present invention, and is not intended to limit the scope of protection of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a solid solution alloy negative electrode material, characterized in that: The steps include: 1) acidifying the carbon nanotubes, then adding the acidified carbon nanotubes and thiourea into water, stirring for 1-2 hours, and removing water by rotary evaporation to obtain a precursor; 2) The precursor prepared in step 1) is kept at 700-800° C. for 3-5 hours in an inert atmosphere to obtain an NC material; 3) mixing the NC material obtained in step 2) with red phosphorus, keeping the mixture at 470-550° C. for 3-6 hours under an inert atmosphere, then cooling the mixture to 230-280° C. for 1-3 hours to obtain a P-NC material; 4) mixing the P-NC material obtained in step 3) with a conductive agent, a binder, and a solvent to prepare a slurry, and then coating the slurry on the surface of the zinc sheet and drying the slurry to obtain a zinc electrode; 5) Using the zinc electrode prepared in step 4) as the working electrode, the Ag / AgCl electrode as the reference electrode, and the carbon rod as the counter electrode, the three-system electrode is subjected to electrodeposition in an electrodeposition solution to obtain; the electrodeposition solution contains zinc ions.

2. The method for preparing a solid solution alloy negative electrode material according to claim 1, characterized in that: In step 1), the mass ratio of carbon nanotubes to thiourea is 0.02-0.03:0.5-2.

3. The method for preparing a solid solution alloy negative electrode material according to claim 1, characterized in that: In step 2), after being kept at 700-800° C. for 3-5 hours, the temperature is lowered, and the mixture is washed with water and ethanol in sequence, and dried in a vacuum oven at 60-80° C. overnight to obtain the NC material.

4. The method for preparing a solid solution alloy negative electrode material according to claim 1, characterized in that: In step 3), the mass ratio of NC material to red phosphorus is 3-5:

1.

5. The method for preparing a solid solution alloy negative electrode material according to claim 1, characterized in that: In step 5), the electrodeposition solution is prepared by adding soluble zinc salt, boric acid, soluble sodium salt and disodium ethylenediaminetetraacetate into water and dissolving them.

6. The method for preparing a solid solution alloy negative electrode material according to any one of claims 1 to 5, characterized in that: The voltage during the electrodeposition in step 5) is 0.8V-2V.

7. The method for preparing a solid solution alloy negative electrode material according to any one of claims 1 to 5, characterized in that: The current density during electrodeposition in step 5) is 20-60 mA cm -2 .

8. The method for preparing a solid solution alloy negative electrode material according to any one of claims 1 to 5, characterized in that: In step 5), the electrodeposition time is 30-300s.

9. A solid solution alloy negative electrode material prepared by the method according to claim 1.

10. Use of the solid solution alloy negative electrode material as claimed in claim 9 in a zinc-air battery.