Ultrahigh molecular weight polyethylene fiber and preparation method thereof
Through polymer blending and modification method, the creep problem of ultra-high molecular weight polyethylene fibers was solved, and fibers suitable for marine engineering were prepared, with excellent creep resistance and comprehensive performance, suitable for marine engineering and deep-sea aquaculture, etc. field.
Patent Information
- Application Number
- CN202411355255.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-15
AI Technical Summary
Ultra-high molecular weight polyethylene fibers are prone to creep under long-term constant loading, especially in high temperature environments, which limits their application in marine engineering and other fields. The existing improved methods such as chemical crosslinking method have poor effect and Difficult to control.
Through the polymer blending and modification method, the specific steps include emulsion of mixed ethylene copolymer and ethylene homopolymer for emulsion, heating and dissolution, extrusion cooling, extraction and drying, and thermal drafting to form an ultra-high molecular weight with excellent comprehensive properties Polyethylene fibers reduce molecular slippage and improve creep resistance.
The prepared fibers meet the requirements of breaking strength and modulus, have significant creep resistance, and are suitable for marine engineering and deep-sea aquaculture. They have simple process, easy operation, pollution-free, and have broad application prospects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultra-high molecular weight polyethylene fibers, and more specifically, to an ultra-high molecular weight polyethylene fiber and a preparation method thereof. Background Art
[0002] Ultra-high molecular weight polyethylene fiber is widely used in mooring ropes, reinforcement of composite materials, medical equipment, cargo nets and other fields due to its light weight and high strength. It has excellent UV resistance, chemical resistance, cut resistance and abrasion resistance.
[0003] However, ultra-high molecular weight polyethylene fiber has a disadvantage. Due to the relatively weak force between macromolecular chains, under the action of long-term constant load, the molecular chains will slip, which is manifested as the gradual elongation of the fiber on a macro scale. The higher the ambient temperature, the faster the elongation. This phenomenon seriously restricts the application of ultra-high molecular weight polyethylene fiber in fields such as marine engineering. This disadvantage is related to its creep behavior.
[0004] Therefore, an ultra-high molecular weight polyethylene fiber with improved creep behavior is needed. Currently, the creep resistance of fibers is generally improved by chemical crosslinking, high-energy radiation crosslinking or raw material modification, but the disadvantages are poor crosslinking effect, poor controllability, or high technical difficulty. Summary of the invention
[0005] In view of this, the object of the present invention is to provide an ultra-high molecular weight polyethylene fiber and a preparation method thereof. The preparation method provided by the present invention can reduce molecular slippage and improve the anti-creep behavior of the fiber through polymer blending modification; the prepared ultra-high molecular weight polyethylene fiber has excellent comprehensive performance, and has good anti-creep performance when the breaking strength and modulus meet the requirements, and is suitable for application in special fields such as marine engineering and deep-sea aquaculture.
[0006] The present invention provides a method for preparing ultra-high molecular weight polyethylene fiber, comprising the following steps:
[0007] a) mixing an emulsion of an ethylene copolymer and an emulsion of an ethylene homopolymer, emulsifying the mixture, and obtaining a mixed solution; the ethylene copolymer is obtained by copolymerization of ethylene and α-olefin; the ethylene homopolymer is ultra-high molecular weight polyethylene;
[0008] b) heating and dissolving the mixed solution obtained in step a) to obtain a spinning melt; then sequentially extruding and cooling the spinning melt to obtain a gel fiber; finally sequentially extracting, drying and heat-drawing the gel fiber to obtain an ultra-high molecular weight polyethylene fiber.
[0009] Preferably, the viscosity average molecular weight of the ethylene copolymer is 1 million to 10 million; and the molecular weight of the ultra-high molecular weight polyethylene is ≥ 6 million.
[0010] Preferably, the ethylene copolymer emulsion in step a) is prepared from ethylene copolymer and white oil, and has a solid content of 5% to 10%;
[0011] The ethylene homopolymer emulsion is prepared from ethylene homopolymer and white oil, and has a solid content of 5% to 10%.
[0012] Preferably, the emulsification temperature in step a) is 60° C. to 80° C., the rotation speed is 1000 r / min to 1500 r / min, and the time is 5 min to 20 min.
[0013] Preferably, in the mixed solution in step a), the proportion of the ethylene copolymer relative to the total mass of the ethylene copolymer and the ethylene homopolymer is ≥ 25%.
[0014] Preferably, the heating and dissolving process in step b) uses a twin-screw extruder with a screw diameter of 90 mm to 160 mm, a screw speed of 100 r / min to 300 r / min, and a screw temperature of 110° C. to 300° C.
[0015] Preferably, the extrusion process in step b) uses a spinneret, and the spinneret has 100 to 400 holes and a hole diameter of 0.5 mm to 1.5 mm;
[0016] The cooling process uses a water tank, and the water temperature in the water tank is 15°C~30°C.
[0017] Preferably, the extraction agent used in the extraction process in step b) is a hydrocarbon cleaning agent, dichloromethane or tetrachloroethylene;
[0018] The extraction also includes:
[0019] The frozen fibers are pre-stretched after being allowed to stand in equilibrium for 20 to 30 hours.
[0020] Preferably, the process of heat stretching in step b) is specifically as follows:
[0021] Level 1 hot stretching, 135℃~140℃; level 2 hot stretching, 142℃~148℃; level 3 hot stretching, 150℃~155℃, the total stretching multiple is 40 times~60 times.
[0022] The present invention also provides an ultra-high molecular weight polyethylene fiber, which is prepared by the preparation method described in the above technical solution.
[0023] The present invention provides an ultra-high molecular weight polyethylene fiber and a preparation method thereof; the preparation method comprises the following steps: a) mixing an emulsion of an ethylene copolymer with an emulsion of an ethylene homopolymer, emulsifying, and obtaining a mixed solution; the ethylene copolymer is formed by copolymerization of ethylene and α-olefin; the ethylene homopolymer is an ultra-high molecular weight polyethylene; b) heating and dissolving the mixed solution obtained in step a) to obtain a spinning melt; then the spinning melt is sequentially extruded and cooled to obtain a gel fiber; finally, the gel fiber is sequentially extracted, dried, and heat-stretched to obtain an ultra-high molecular weight polyethylene fiber. Compared with the prior art, the preparation method provided by the present invention selects specific raw material components and specific process steps to achieve overall better interaction: through polymer blending modification, molecular slip can be reduced and the creep resistance of the fiber can be improved; the prepared ultra-high molecular weight polyethylene fiber has excellent comprehensive performance, and has good creep resistance when the breaking strength and modulus meet the requirements, and is suitable for application in special fields such as marine engineering and deep-sea aquaculture.
[0024] At the same time, the preparation method provided by the present invention has simple process, easy-to-operate steps, mild and easy-to-control conditions, no pollution, and has broad application prospects. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention provides a method for preparing ultra-high molecular weight polyethylene fiber, comprising the following steps:
[0027] a) mixing an emulsion of an ethylene copolymer and an emulsion of an ethylene homopolymer, emulsifying the mixture, and obtaining a mixed solution; the ethylene copolymer is obtained by copolymerization of ethylene and α-olefin; the ethylene homopolymer is ultra-high molecular weight polyethylene;
[0028] b) heating and dissolving the mixed solution obtained in step a) to obtain a spinning melt; then sequentially extruding and cooling the spinning melt to obtain a gel fiber; finally sequentially extracting, drying and heat-drawing the gel fiber to obtain an ultra-high molecular weight polyethylene fiber.
[0029] The present invention firstly mixes the emulsion of ethylene copolymer and the emulsion of ethylene homopolymer, and emulsifies them to obtain a mixed solution.
[0030] In the present invention, the ethylene copolymer is formed by copolymerization of ethylene and α-olefin, wherein the proportion of α-olefin is preferably 0.1 mol% to 1 mol%; the α-olefin is preferably selected from one or more of 1-butene, 1-hexene, and 1-octene, more preferably 1-butene or 1-hexene.
[0031] In the present invention, the viscosity average molecular weight of the ethylene copolymer is preferably 1 million to 10 million, more preferably 3 million to 5 million.
[0032] In the present invention, the ethylene homopolymer is ultra-high molecular weight polyethylene; the molecular weight of the ultra-high molecular weight polyethylene is preferably ≥ 6 million, more preferably ≥ 8 million.
[0033] The present invention has no particular limitation on the sources of the ethylene copolymer and ethylene homopolymer, and any commercially available product or self-made product known to those skilled in the art may be used.
[0034] In the present invention, the emulsion of the ethylene copolymer is preferably prepared from an ethylene copolymer and white oil, and the solid content is preferably 5% to 10%; the emulsion of the ethylene homopolymer is preferably prepared from an ethylene homopolymer and white oil, and the solid content is 5% to 10%.
[0035] In the present invention, the emulsification method is preferably high-speed emulsification; the emulsification temperature is preferably 60°C~80°C, more preferably 65°C~75°C, the rotation speed is preferably 1000r / min~1500r / min, more preferably 1200r / min~1300r / min, and the time is preferably 5min~20min, more preferably 10min~15min.
[0036] In the present invention, in the mixed solution, the proportion of the ethylene copolymer to the total mass of the ethylene copolymer and the ethylene homopolymer is preferably ≥25%, specifically 25%, 50%, 75%, 90%.
[0037] After obtaining the mixed solution, the present invention heats and dissolves the mixed solution to obtain a spinning melt; then the spinning melt is sequentially extruded and cooled to obtain a gel fiber; finally, the gel fiber is sequentially extracted, dried and heat-stretched to obtain an ultra-high molecular weight polyethylene fiber.
[0038] In the present invention, the heating and dissolving process preferably uses a twin-screw extruder, the screw diameter is preferably 90mm~160mm, more preferably 95mm~96mm, the screw speed is preferably 100r / min~300r / min, more preferably 150r / min~250r / min, and the screw temperature is preferably 110℃~300℃, more preferably 118℃~287℃.
[0039] In the present invention, the extrusion process preferably uses a spinneret, and the spinneret preferably has 100 to 400 holes, more preferably 240 to 250 holes, and the pore size is preferably 0.5 mm to 1.5 mm, more preferably 1 mm.
[0040] In the present invention, the cooling process preferably uses a water tank, and the water temperature in the water tank is preferably 15°C~30°C, more preferably 25°C; after cooling, it is shaped into frozen gel filaments, and subsequently subjected to extraction and drying treatment and multiple heat stretching processes to obtain ultra-high molecular weight polyethylene fibers.
[0041] In the present invention, the extractant used in the extraction process is preferably a hydrocarbon cleaning agent, dichloromethane or tetrachloroethylene; commercially available products well known to those skilled in the art can be used.
[0042] In the present invention, the extraction preferably further comprises:
[0043] The frozen gel fibers are allowed to stand for 20 to 30 hours before being pre-stretched;
[0044] More preferably:
[0045] The gel fibers were pre-stretched after being allowed to stand in equilibrium for 24 hours.
[0046] In the present invention, the process of heat drawing is preferably as follows:
[0047] 1st level heat drawing, 135℃~140℃; 2nd level heat drawing, 142℃~148℃; 3rd level heat drawing, 150℃~155℃, the total drawing multiple is 40 times~60 times;
[0048] More preferably:
[0049] Level 1 hot stretching, 137°C; level 2 hot stretching, 148°C; level 3 hot stretching, 150°C, the total stretching multiple is 50 times.
[0050] The preparation method provided by the invention has simple process, easy-to-operate steps, mild and easy-to-control conditions, no pollution, and broad application prospects.
[0051] The present invention also provides an ultra-high molecular weight polyethylene fiber, which is prepared by the preparation method described in the above technical solution. In the present invention, the ultra-high molecular weight polyethylene fiber is mainly composed of component A and component B, wherein component A is an ethylene copolymer, component B is an ethylene homopolymer, and the mass proportion of component A (relative to the total mass of component A and component B) is ≥25%; the preparation method provided by the present invention selects the above-mentioned specific raw material components and cooperates with specific process steps to achieve overall good interaction: through polymer blending modification, molecular slip can be reduced and the anti-creep behavior of the fiber can be improved; the prepared ultra-high molecular weight polyethylene fiber has excellent comprehensive performance, and has good anti-creep performance when the breaking strength and modulus meet the requirements, and is suitable for application in special fields such as marine engineering and deep-sea aquaculture. The experimental results show that the breaking strength of the ultra-high molecular weight polyethylene fiber provided by the present invention is ≥22cN / dtex, and the modulus is ≥750cN / dtex; the creep elongation of the fiber at 70°C and 10% load for 100h is ≤7%.
[0052] The present invention provides an ultra-high molecular weight polyethylene fiber and a preparation method thereof; the preparation method comprises the following steps: a) mixing an emulsion of an ethylene copolymer with an emulsion of an ethylene homopolymer, emulsifying, and obtaining a mixed solution; the ethylene copolymer is formed by copolymerization of ethylene and α-olefin; the ethylene homopolymer is an ultra-high molecular weight polyethylene; b) heating and dissolving the mixed solution obtained in step a) to obtain a spinning melt; then the spinning melt is sequentially extruded and cooled to obtain a gel fiber; finally, the gel fiber is sequentially extracted, dried, and heat-stretched to obtain an ultra-high molecular weight polyethylene fiber. Compared with the prior art, the preparation method provided by the present invention selects specific raw material components and specific process steps to achieve overall better interaction: through polymer blending modification, molecular slip can be reduced and the creep resistance of the fiber can be improved; the prepared ultra-high molecular weight polyethylene fiber has excellent comprehensive performance, and has good creep resistance when the breaking strength and modulus meet the requirements, and is suitable for application in special fields such as marine engineering and deep-sea aquaculture.
[0053] At the same time, the preparation method provided by the present invention has simple process, easy-to-operate steps, mild and easy-to-control conditions, no pollution, and has broad application prospects.
[0054] In order to further illustrate the present invention, the following examples are provided for detailed description. The raw materials used in the following examples of the present invention are all commercially available.
[0055] Example 1
[0056] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, mainly composed of component A and component B, wherein component A is an ethylene-1-butene copolymer (viscosity average molecular weight 4 million, 1-butene accounts for 0.5 mol%), and component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 8 million; the preparation method comprises the following steps:
[0057] (1) Component A and white oil are prepared into a mixed emulsion AA having a solid content of 8%;
[0058] (2) Component B and white oil are prepared into a mixed emulsion BB with a solid content of 8%;
[0059] (3) Mixing the mixed emulsion AA and the mixed emulsion BB in a weight ratio of 25:75, at 70°C and a high-speed emulsifier of 1200 r / min for 10 min to obtain a mixed solution CC, in which component A accounts for 25% of the total weight of component A and component B;
[0060] (4) The mixed liquid CC is heated and dissolved (twin-screw extruder, screw diameter 96 mm, screw speed 200 r / min, screw zone 1-16 temperatures are 118°C, 154°C, 225°C, 257°C, 259°C, 272°C, 273°C, 275°C, 277°C, 278°C, 279°C, 279°C, 281°C, 283°C, 285°C, 287°C) to prepare a spinning melt; then, an extrusion and cooling device is used to prepare jelly silk, and the jelly silk is subjected to extraction and drying treatment. And multiple heat stretching is carried out (specifically: the spinning melt is measured by a metering pump and extruded through a spinneret, the spinneret has 240 holes and a hole diameter of 1.0 mm, and is cooled and shaped in a water tank (water temperature 25°C) to obtain frozen gel fibers. After the frozen gel fibers are balanced and stood for 24 hours, they are pre-stretched, extracted (the extractant is a hydrocarbon cleaning agent), dried, and hot stretched (1st level hot stretching (137°C), 2nd level hot stretching (148°C), 3rd level hot stretching (150°C), and the total stretching multiple is 50 times)) to obtain ultra-high molecular weight polyethylene fibers.
[0061] According to the test, the creep elongation of the ultra-high molecular weight polyethylene fiber is 4.40% at 70°C and 10% load after 100h.
[0062] Example 2
[0063] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, mainly composed of component A and component B, wherein component A is a copolymer of ethylene and 1-hexene (viscosity average molecular weight 4 million, 1-hexene accounts for 0.4 mol%), and component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 8 million; the preparation method is as described in Example 1, wherein in step (3), component A in the mixed solution accounts for 25% of the total mass of component A and component B.
[0064] According to the test, the creep elongation of the ultra-high molecular weight polyethylene fiber at 70°C and 10% load after 100 hours is 3.64%.
[0065] Example 3
[0066] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, mainly composed of component A and component B, wherein component A is a copolymer of ethylene and 1-hexene (viscosity average molecular weight 4 million, 1-hexene accounts for 0.4 mol%), and component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 8 million; the preparation method is as described in Example 1, wherein in step (3), component A in the mixed solution accounts for 50% of the total mass of component A and component B.
[0067] According to the test, the creep elongation of the ultra-high molecular weight polyethylene fiber at 70°C and 10% load after 100 hours is 1.72%.
[0068] Example 4
[0069] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, mainly composed of component A and component B, wherein component A is a copolymer of ethylene and 1-hexene (viscosity average molecular weight 4 million, 1-hexene accounts for 0.4 mol%), and component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 9.8 million; the preparation method is as described in Example 1, wherein in step (3), component A in the mixed solution accounts for 75% of the total mass of component A and component B.
[0070] According to the test, the creep elongation of the ultra-high molecular weight polyethylene fiber at 70°C and 10% load after 100 hours is 0.05%.
[0071] Example 5
[0072] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, mainly composed of component A and component B, wherein component A is a copolymer of ethylene and 1-hexene (viscosity average molecular weight 4 million, 1-hexene accounts for 0.4 mol%), and component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 8 million; the preparation method is as described in Example 1, wherein in step (3), component A in the mixed solution accounts for 90% of the total mass of component A and component B.
[0073] According to the test, the creep elongation of the ultra-high molecular weight polyethylene fiber at 70°C and 10% load after 100 hours is 0.25%.
[0074] Comparative Example 1
[0075] An ultra-high molecular weight polyethylene fiber and a preparation method thereof, comprising component B, wherein component B is an ethylene homopolymer, and the homopolymer is an ultra-high molecular weight polyethylene with a molecular weight of 8 million; the preparation method is as described in Example 1 (omitting the steps involving component A).
[0076] According to tests, the creep elongation of the ultra-high molecular weight polyethylene fiber is greater than 10% at 70°C and 10% load for 100 hours.
[0077] The composition, proportion and performance data of the above ultra-high molecular weight polyethylene fibers are shown in Table 1 below.
[0078] Table 1
[0079]
[0080] As can be seen from Table 1, the ultra-high molecular weight polyethylene fiber provided by the present invention can reduce molecular slippage and improve the creep resistance of the fiber through polymer blending modification; compared with conventional ultra-high molecular weight polyethylene fibers, the ultra-high molecular weight polyethylene fibers provided by the present invention have good dimensional stability at a temperature of 70°C and a load of 10% on the basis of good and stable performance; therefore, the ultra-high molecular weight polyethylene fiber prepared by the present invention has excellent comprehensive performance, and has good creep resistance when the breaking strength and modulus meet the requirements, and is suitable for application in special fields such as marine engineering and deep-sea aquaculture; at the same time, the preparation method provided by the present invention has a simple process, mild conditions, easy control, is convenient for industrial production, and has broad application prospects.
[0081] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing ultra-high molecular weight polyethylene fiber, comprising the following steps: a) mixing an emulsion of an ethylene copolymer and an emulsion of an ethylene homopolymer, emulsifying the mixture, and obtaining a mixed solution; the ethylene copolymer is obtained by copolymerization of ethylene and α-olefin; the ethylene homopolymer is ultra-high molecular weight polyethylene; b) heating and dissolving the mixed solution obtained in step a) to obtain a spinning melt; then sequentially extruding and cooling the spinning melt to obtain a gel fiber; finally sequentially extracting, drying and heat-drawing the gel fiber to obtain an ultra-high molecular weight polyethylene fiber.
2. The preparation method according to claim 1, characterized in that: The viscosity average molecular weight of the ethylene copolymer is 1 million to 10 million; the molecular weight of the ultra-high molecular weight polyethylene is ≥ 6 million.
3. The preparation method according to claim 1, characterized in that: The ethylene copolymer emulsion in step a) is prepared from ethylene copolymer and white oil, and has a solid content of 5% to 10%; The ethylene homopolymer emulsion is prepared from ethylene homopolymer and white oil, and has a solid content of 5% to 10%.
4. The preparation method according to claim 1, characterized in that: The emulsification temperature in step a) is 60° C. to 80° C., the rotation speed is 1000 r / min to 1500 r / min, and the time is 5 min to 20 min.
5. The preparation method according to claim 1, characterized in that: In the mixed solution in step a), the proportion of the ethylene copolymer to the total mass of the ethylene copolymer and the ethylene homopolymer is ≥25%.
6. The preparation method according to claim 1, characterized in that: The heating and dissolving process in step b) uses a twin-screw extruder with a screw diameter of 90 mm to 160 mm, a screw speed of 100 r / min to 300 r / min, and a screw temperature of 110° C. to 300° C.
7. The preparation method according to claim 1, characterized in that: The extrusion process in step b) uses a spinneret, wherein the spinneret has 100 to 400 holes and a hole diameter of 0.5 mm to 1.5 mm; The cooling process uses a water tank, and the water temperature in the water tank is 15°C~30°C.
8. The preparation method according to claim 1, characterized in that: The extraction agent used in the extraction process in step b) is a hydrocarbon cleaning agent, dichloromethane or tetrachloroethylene; The extraction also includes: The frozen fibers are pre-stretched after being allowed to stand in equilibrium for 20 to 30 hours.
9. The preparation method according to claim 1, characterized in that: The process of heat drawing in step b) is specifically as follows: Level 1 hot stretching, 135℃~140℃; level 2 hot stretching, 142℃~148℃; level 3 hot stretching, 150℃~155℃, the total stretching multiple is 40 times~60 times.
10. An ultra-high molecular weight polyethylene fiber, characterized in that: The method is prepared by any one of claims 1 to 9.