Flame-retardant covering yarn and preparation method thereof
By using aramid fiber as the core layer and flame retardant polyester fiber and flame retardant viscose fiber in the flame retardant core yarn, combined with high-efficiency flame retardant, the flame retardant core yarn in the prior art is solved under extreme conditions in the prior art The problem of uneven structural support and flame retardant effect achieves a higher balance of flame retardant performance and mechanical properties.
Patent Information
- Application Number
- CN202411303478.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing flame retardant core yarns have shortcomings in the selection of core layer materials and the distribution of flame retardant, resulting in poor structural support under extreme conditions and uneven flame retardant effects, making it difficult to meet market demand and safety standards.
Aramid fiber is used as the core layer, combined with flame-retardant polyester fiber and flame-retardant viscose fiber, and a heat-insulating and oxygen-insulating protective layer is formed through uniform dispersion of high-efficiency flame retardant to enhance flame retardant performance.
It achieves a good balance between flame retardant performance and mechanical properties, softness, moisture absorption and breathability, and can show excellent flame retardant performance in the ultimate oxygen index and vertical combustion test, providing more reliable protection for personnel and property.
Smart Images

Figure BDA0005048385590000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, in particular to a flame-retardant core-spun yarn and a preparation method thereof. Background Art
[0002] Flame-retardant core-spun yarn is a functional yarn widely used in the textile industry. It is mainly used to produce flame-retardant fabrics and is suitable for fire protection, petrochemical, aerospace and other fields. With the improvement of safety awareness and the continuous improvement of laws and regulations, the market demand for flame-retardant fabrics is growing. In order to meet this demand, researchers are constantly exploring new flame-retardant technologies and materials to improve the safety performance and service life of flame-retardant core-spun yarn.
[0003] At present, in the selection of core layer materials for existing flame-retardant core-spun yarns, common fibers often perform poorly in terms of high temperature resistance and high strength, and cannot provide stable structural support for the core-spun yarn under extreme conditions. The flame-retardant fibers used in the cortex are not uniform in the addition and distribution of flame retardants, resulting in uneven flame retardant effects and difficulty in achieving ideal flame retardant standards. At the same time, due to material and process limitations, existing flame-retardant core-spun yarns are difficult to achieve a good balance in terms of mechanical properties, softness, moisture absorption and air permeability, affecting their comfort and applicability in actual use.
[0004] In summary, the existing flame-retardant core-spun yarn technology has obvious defects in material selection, preparation process and performance, and cannot meet the growing market demand and strict safety standards. Therefore, the development of an innovative material combination and optimized preparation method to achieve the production of high-performance flame-retardant core-spun yarn has become an important issue that needs to be urgently solved in the current textile technology field. Summary of the invention
[0005] Technical issues solved
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a flame-retardant core-spun yarn and a preparation method thereof. By adopting aramid fiber as the core layer, the aramid fiber itself has excellent high temperature resistance and flame retardant properties. The skin layer is blended by flame-retardant polyester fiber and flame-retardant viscose fiber. The two fibers work synergistically to effectively prevent the spread of flames.
[0007] Technical Solution
[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0009] On the one hand, a flame retardant core-spun yarn is composed of a core layer and a skin layer, specifically comprising:
[0010] The core layer is made of aramid fiber, which is para-aramid, i.e. poly(p-phenylene terephthalamide) fiber, which has extremely high molecular chain regularity and crystallinity, giving it excellent high temperature resistance, and its high strength and high modulus provide inner core support for the core-spun yarn;
[0011] The skin layer is made of a blend of flame-retardant polyester fiber and flame-retardant viscose fiber;
[0012] The flame retardant polyester fiber is composed of polyester chips and flame retardants. The polyester chips are polyethylene terephthalate (PET) chips. The added flame retardants include organic phosphorus flame retardants and inorganic flame retardants, namely phosphate compounds and aluminum hydroxide. These flame retardants are uniformly dispersed in the polyester matrix through chemical reactions, and form a heat-insulating and oxygen-isolating protective layer during combustion, thereby preventing the spread of flames.
[0013] The flame retardant viscose fiber comprises viscose stock solution and flame retardant. The viscose stock solution is obtained by chemically treating natural cellulose. The flame retardant used is the same as that in the flame retardant polyester fiber, including organic and inorganic types.
[0014] Furthermore, the aramid fiber used in the core layer has a fineness of 1.5D and a fiber length of 38mm. The breaking strength of the aramid fiber is 20cN / Tex and the breaking elongation is 2.5%, which makes the core layer have excellent resistance to tensile force.
[0015] Furthermore, the organic phosphorus flame retardant in the skin layer achieves a flame retardant effect by promoting the carbonization of polyester and making the carbon layer stable and dense, while the inorganic flame retardant exerts a flame retardant effect by decomposing, absorbing heat and diluting combustible gases.
[0016] Furthermore, the mass ratio of polyester chips to flame retardant in the flame retardant polyester fiber is 100:12. When the addition amount of the flame retardant is 10, the afterburning time of the flame retardant polyester fiber in the vertical combustion test can be shortened to 2s, and the damaged length is reduced to 10cm. When the addition amount reaches 15, its limiting oxygen index is increased to 32%, showing more excellent flame retardant properties.
[0017] Furthermore, in the flame retardant viscose fiber, the mass ratio of viscose stock solution to flame retardant is 100:10. When the addition amount of flame retardant is 8, the initial decomposition temperature of the fiber in thermogravimetric analysis increases by 50°C. When the addition amount reaches 12, the peak value of the heat release rate in the cone calorimeter test decreases by 30kW / m 2 , suppressing the intensity of combustion.
[0018] On the other hand, a method for preparing a flame retardant core-spun yarn is provided, wherein the specific steps of the preparation method are:
[0019] S1. Preparation of flame retardant polyester fiber:
[0020] S1.1, Slice drying: Place the polyester slices in a vacuum drying oven for deep drying, using the vacuum environment to remove moisture;
[0021] S1.2, co-extrusion: add the dried polyester chips and flame retardant into the twin-screw extruder, divide the heating area of the extruder, and under the high temperature and the shearing and mixing action of the twin screws, the polyester chips and the flame retardant are fully blended;
[0022] S1.3, spinning molding: the prepared flame retardant polyester chips are converted into flame retardant polyester fibers through a spinning process. During the spinning process, the spinning speed is controlled at 1000-1200 m / min, and the stretching multiple is set to 3-5 times, so that the fiber fineness reaches 1.5-2.0 dtex.
[0023] S2. Preparation of flame retardant viscose fiber:
[0024] S2.1, stock solution preparation: fully mix the viscose stock solution and the flame retardant, and monitor the temperature and viscosity changes of the solution in real time during the mixing process;
[0025] S2.2, precision spinning: the prepared mixed solution is filtered to remove impurities and undissolved particles, the filtered solution is extruded through a spinneret to form filaments, the spinneret has an aperture of 0.1-0.2 mm and 80-150 holes, the filaments are coagulated in a coagulation bath, the coagulated filaments are washed, desulfurized, oiled, and stretched with a stretching multiple of 2-3 times, and wound to obtain flame-retardant viscose fibers.
[0026] S3. Preparation of flame retardant core-spun yarn:
[0027] S3.1, core layer introduction: select aramid fiber with a fineness of 1.5D and a length of 38mm as the core layer, and introduce the aramid fiber into the twisting area of the spinning machine through the wire guide device;
[0028] S3.2, skin coating molding: the flame retardant polyester fiber and the flame retardant viscose fiber are fully mixed in a mass ratio of 60:40, and the mixed fibers are fed into the twisting area of the spinning machine to be coated and twisted with the core layer fibers. The spindle speed of the spinning machine is controlled at 8000-10000 rpm to obtain the flame retardant core-spun yarn.
[0029] Furthermore, in S1.1, the polyester chips are placed in a vacuum drying oven and dried at a temperature of 120-130° C. for 8-10 hours. During this process, the chips are turned over every 2 hours to reduce the water content of the chips to 0.01%.
[0030] Furthermore, in step S1.2, the fully dried polyester chips and the flame retardant are added into a twin-screw extruder in a mass ratio of 100:15, and the temperature of each section of the twin-screw extruder is set to: 250°C in zone 1, 260°C in zone 2, 270°C in zone 3, and 280°C in zone 4. During the extrusion process, the screw speed is controlled at 200-300 rpm, so that the polyester chips and the flame retardant are fully melted and blended, and evenly dispersed to form a polyester melt with flame retardant properties.
[0031] Furthermore, the S2.1 detects the viscose stock solution, puts the viscose stock solution into a stirring kettle, slowly adds the flame retardant into the viscose stock solution at a mass ratio of 100:12 under a stirring speed of 100-150 rpm, and continues stirring for 2-3 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution.
[0032] Furthermore, the S2.2 coagulation bath adopts a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid is controlled at 120-150 g / L, the concentration of sodium sulfate is 250-300 g / L, the concentration of zinc sulfate is 5-10 g / L, and the temperature is controlled at 45-55°C.
[0033] Beneficial Effects
[0034] Compared with the known public technology, the technical solution provided by the present invention has the following advantages:
[0035] Beneficial effects:
[0036] 1. The present invention adopts aramid fiber as the core layer, and the skin layer is blended by flame-retardant polyester fiber and flame-retardant viscose fiber. After adding high-efficiency flame retardant, these two fibers are blended through a blending process, so that the flame retardant is more evenly distributed in the fiber, and the synergistic effect is enhanced. During combustion, an effective heat-insulating and oxygen-isolating protective layer can be quickly formed to prevent the spread of flames. The flame-retardant core-spun yarn of the present invention can maintain good flame-retardant properties for a longer time and in a more severe fire environment in terms of limiting oxygen index and vertical burning test, thereby buying more precious time for personnel escape and property protection.
[0037] 2. The flame-retardant core-spun yarn of the present invention successfully achieves a good balance between flame-retardant properties and comprehensive properties of mechanical properties, softness, and moisture absorption and breathability. Aramid fiber as the core layer provides high strength and high modulus, ensuring the mechanical properties of the yarn. The reasonable blending of flame-retardant polyester fiber and flame-retardant viscose fiber in the cortex improves the softness and moisture absorption and breathability of the yarn while maintaining the flame-retardant effect. This makes the flame-retardant core-spun yarn of the present invention not only suitable for professional protection fields with extremely high requirements for flame-retardant properties, but also can be used in civilian fields with certain requirements for comfort, broadening its scope of application. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the present invention is described clearly and completely. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] The present invention will be further described below in conjunction with the embodiments.
[0040] Embodiment 1
[0041] This embodiment describes in detail a specific process of a method for preparing a flame-retardant core-spun yarn, and displays in detail specific preparation parameters and performance test data to verify the effectiveness and superiority of the invention.
[0042] Preparation of flame-retardant polyester fiber: Put the polyester chips into a vacuum drying oven, dry them at a temperature of 125°C for 9 hours, turn the chips every 2 hours to reduce the moisture content of the chips to 0.01%, and add the fully dried polyester chips and the flame retardant into a twin-screw extruder according to a mass ratio of 100:12. The temperature of each section of the twin-screw extruder is set to: 250°C in zone 1, 260°C in zone 2, 270°C in zone 3, and 280°C in zone 4. During the extrusion process, the screw speed is controlled at 250 rpm to fully melt and blend the polyester chips and the flame retardant, and evenly disperse them to form a polyester melt with flame retardant properties. The prepared flame-retardant polyester chips are converted into flame-retardant polyester fibers through a spinning process. The spinning speed is controlled at 1100m / min and the stretching multiple is set to 4 times, so that the fiber fineness reaches 1.8dtex.
[0043] Preparation of flame-retardant viscose fiber: The viscose stock solution was tested, and the viscose stock solution was put into a stirring kettle. Under the condition of a stirring speed of 120 rpm, the flame retardant was slowly added to the viscose stock solution at a mass ratio of 100:10, and the stirring was continued for 2.5 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution. The prepared mixed solution was filtered to remove impurities and undissolved particles therein, and the filtered solution was extruded through a spinneret to form filaments. The spinneret had an aperture of 0.15 mm and 120 holes. The filaments were coagulated and formed in a coagulation bath. The coagulation bath used a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid was controlled at 130 g / L, the concentration of sodium sulfate was 280 g / L, the concentration of zinc sulfate was 8 g / L, and the temperature was controlled at 50°C. The coagulated filaments were washed, desulfurized, oiled, and drawn at a drawing multiple of 2.5 times, and wound to obtain flame-retardant viscose fibers.
[0044] Preparation of flame-retardant core-spun yarn: Aramid fiber with a fineness of 1.5D and a length of 38 mm was selected as the core layer, the aramid fiber was introduced into the twisting area of the spinning machine through a wire guide device, the flame-retardant polyester fiber and the flame-retardant viscose fiber were fully mixed in a mass ratio of 60:40, and the mixed fibers were sent into the twisting area of the spinning machine for coating and twisting with the core layer fibers. The spindle speed of the spinning machine was controlled at 9000 rpm to obtain the flame-retardant core-spun yarn.
[0045] The flame retardant core-spun yarn prepared in this embodiment was tested for performance, and its breaking strength was 19.5 cN / Tex, the breaking elongation was 12.8%, the limiting oxygen index was 31.5%, the afterflaming time in the vertical burning test was 1.8 s, and the damaged length was 9 cm.
[0046] Embodiment 2
[0047] Preparation of flame-retardant polyester fiber: Put the polyester slices into a vacuum drying oven, dry them at a temperature of 130° C. for 8 hours, turn the slices over every 2 hours to reduce the moisture content of the slices to 0.01%, add the fully dried polyester slices and the flame retardant into a twin-screw extruder according to a mass ratio of 100:15, and set the temperature of each section of the twin-screw extruder to: 250° C. in the first zone, 260° C. in the second zone, 270° C. in the third zone, and 280° C. in the fourth zone. During the extrusion process, the screw speed is controlled at 300 rpm, so that the polyester slices and the flame retardant are fully melt-blended and evenly dispersed to form a polyester melt with flame-retardant properties. The prepared flame-retardant polyester slices are converted into flame-retardant polyester fibers through a spinning process, the spinning speed is controlled at 1200 m / min, and the stretching multiple is set to 5 times, so that the fiber fineness reaches 2.0 dtex.
[0048] Preparation of flame-retardant viscose fiber: The viscose stock solution was tested, and the viscose stock solution was put into a stirring kettle. Under the condition of a stirring speed of 150 rpm, the flame retardant was slowly added to the viscose stock solution at a mass ratio of 100:12, and the stirring was continued for 3 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution. The prepared mixed solution was filtered to remove impurities and undissolved particles therein, and the filtered solution was extruded through a spinneret to form filaments. The spinneret had an aperture of 0.2 mm and 150 holes. The filaments were coagulated and formed in a coagulation bath. The coagulation bath used a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid was controlled at 150 g / L, the concentration of sodium sulfate was 300 g / L, the concentration of zinc sulfate was 10 g / L, and the temperature was controlled at 55°C. The coagulated filaments were washed, desulfurized, oiled, and drawn, and the drawing multiple was 3 times, and wound to obtain flame-retardant viscose fibers.
[0049] Preparation of flame-retardant core-spun yarn: Aramid fiber with a fineness of 1.5D and a length of 38 mm was selected as the core layer, the aramid fiber was introduced into the twisting area of the spinning machine through a wire guide device, the flame-retardant polyester fiber and the flame-retardant viscose fiber were fully mixed in a mass ratio of 60:40, and the mixed fibers were sent into the twisting area of the spinning machine for coating and twisting with the core layer fibers. The spindle speed of the spinning machine was controlled at 10,000 rpm to obtain the flame-retardant core-spun yarn.
[0050] The flame retardant core-spun yarn prepared in this embodiment was tested for performance, and its breaking strength was 20.2 cN / Tex, the breaking elongation was 13.2%, the limiting oxygen index was 32.8%, the afterflaming time in the vertical burning test was 1.5 s, and the damaged length was 8 cm.
[0051] Embodiment 3
[0052] Preparation of flame-retardant polyester fiber: Put the polyester slices into a vacuum drying oven, dry them at a temperature of 120° C. for 10 hours, turn the slices every 2 hours to reduce the moisture content of the slices to 0.01%, add the fully dried polyester slices and the flame retardant into a twin-screw extruder according to a mass ratio of 100:10, and set the temperature of each section of the twin-screw extruder to: 250° C. in the first zone, 260° C. in the second zone, 270° C. in the third zone, and 280° C. in the fourth zone. During the extrusion process, the screw speed is controlled at 200 rpm, so that the polyester slices and the flame retardant are fully melt-blended and evenly dispersed to form a polyester melt with flame-retardant properties. The prepared flame-retardant polyester slices are converted into flame-retardant polyester fibers through a spinning process, the spinning speed is controlled at 1000 m / min, and the stretching multiple is set to 3 times, so that the fiber fineness reaches 1.5 dtex.
[0053] Preparation of flame-retardant viscose fiber: testing the viscose stock solution, putting the viscose stock solution into a stirring kettle, slowly adding the flame retardant to the viscose stock solution at a mass ratio of 100:8 under the condition of a stirring speed of 100 rpm, and continuously stirring for 2 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution, filtering the prepared mixed solution to remove impurities and undissolved particles therein, and extruding the filtered solution through a spinneret to form filaments, the spinneret having an aperture of 0.1 mm and 80 holes, and the filaments are coagulated and formed in a coagulation bath, and the coagulation bath adopts a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid is controlled at 120 g / L, the concentration of sodium sulfate is 250 g / L, the concentration of zinc sulfate is 5 g / L, and the temperature is controlled at 45°C, and the coagulated filaments are washed, desulfurized, oiled, and drawn, the drawing multiple is 2 times, and wound to obtain flame-retardant viscose fiber.
[0054] Preparation of flame-retardant core-spun yarn: Aramid fiber with a fineness of 1.5D and a length of 38 mm was selected as the core layer, and the aramid fiber was introduced into the twisting area of the spinning machine through a wire guide device. The flame-retardant polyester fiber and the flame-retardant viscose fiber were fully mixed in a mass ratio of 60:40, and the mixed fibers were sent into the twisting area of the spinning machine for coating and twisting with the core layer fibers. The spindle speed of the spinning machine was controlled at 8000 rpm to obtain the flame-retardant core-spun yarn.
[0055] The flame retardant core-spun yarn prepared in this embodiment was tested for performance, and its breaking strength was 18.8 cN / Tex, the breaking elongation was 12.0%, the limiting oxygen index was 30.5%, the afterflaming time in the vertical burning test was 2.2 s, and the damaged length was 11 cm.
[0056] Embodiment 4
[0057] Preparation of flame-retardant polyester fiber: Put the polyester slices into a vacuum drying oven, dry them at a temperature of 128° C. for 9 hours, turn the slices every 2 hours to reduce the moisture content of the slices to 0.01%, add the fully dried polyester slices and the flame retardant into a twin-screw extruder according to a mass ratio of 100:14, and set the temperature of each section of the twin-screw extruder to: 250° C. for zone 1, 260° C. for zone 2, 270° C. for zone 3, and 280° C. for zone 4. During the extrusion process, the screw speed is controlled at 280 rpm to fully melt-blend the polyester slices and the flame retardant and evenly disperse them to form a polyester melt with flame-retardant properties. The prepared flame-retardant polyester slices are converted into flame-retardant polyester fibers through a spinning process, the spinning speed is controlled at 1150 m / min, and the stretching multiple is set to 4.5 times, so that the fiber fineness reaches 1.9 dtex.
[0058] Preparation of flame-retardant viscose fiber: The viscose stock solution was tested, and the viscose stock solution was put into a stirring kettle. Under the condition of a stirring speed of 140 rpm, the flame retardant was slowly added to the viscose stock solution at a mass ratio of 100:11, and the stirring was continued for 2.8 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution. The prepared mixed solution was filtered to remove impurities and undissolved particles therein, and the filtered solution was extruded through a spinneret to form filaments. The spinneret had an aperture of 0.18 mm and 140 holes. The filaments were coagulated and formed in a coagulation bath. The coagulation bath used a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid was controlled at 140 g / L, the concentration of sodium sulfate was 290 g / L, the concentration of zinc sulfate was 9 g / L, and the temperature was controlled at 52°C. The coagulated filaments were washed, desulfurized, oiled, and drawn at a drawing multiple of 2.8 times, and wound to obtain flame-retardant viscose fibers.
[0059] Preparation of flame-retardant core-spun yarn: Aramid fiber with a fineness of 1.5D and a length of 38 mm was selected as the core layer, and the aramid fiber was introduced into the twisting area of the spinning machine through a wire guide device. The flame-retardant polyester fiber and the flame-retardant viscose fiber were fully mixed in a mass ratio of 60:40, and the mixed fibers were sent into the twisting area of the spinning machine for coating and twisting with the core layer fibers. The spindle speed of the spinning machine was controlled at 9500 rpm to obtain the flame-retardant core-spun yarn.
[0060] The flame retardant core-spun yarn prepared in this embodiment was tested for performance, and its breaking strength was 19.8 cN / Tex, the breaking elongation was 12.9%, the limiting oxygen index was 32.0%, the afterflaming time in the vertical burning test was 1.7 s, and the damaged length was 9.5 cm.
[0061] Embodiment 5
[0062] Preparation of flame-retardant polyester fiber: Put the polyester slices into a vacuum drying oven, dry them at a temperature of 122° C. for 8.5 hours, turn the slices every 2 hours to reduce the moisture content of the slices to 0.01%, add the fully dried polyester slices and the flame retardant into a twin-screw extruder according to a mass ratio of 100:11, and set the temperature of each section of the twin-screw extruder to: 250° C. for zone 1, 260° C. for zone 2, 270° C. for zone 3, and 280° C. for zone 4. During the extrusion process, the screw speed is controlled at 220 rpm to fully melt-blend the polyester slices and the flame retardant and evenly disperse them to form a polyester melt with flame-retardant properties. The prepared flame-retardant polyester slices are converted into flame-retardant polyester fibers through a spinning process, the spinning speed is controlled at 1050 m / min, and the stretching multiple is set to 3.5 times, so that the fiber fineness reaches 1.6 dtex.
[0063] Preparation of flame-retardant viscose fiber: The viscose stock solution was tested, and the viscose stock solution was put into a stirring kettle. Under the condition of a stirring speed of 110 rpm, the flame retardant was slowly added to the viscose stock solution at a mass ratio of 100:9, and the stirring was continued for 2.2 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution. The prepared mixed solution was filtered to remove impurities and undissolved particles therein, and the filtered solution was extruded through a spinneret to form filaments. The spinneret had an aperture of 0.12 mm and 100 holes. The filaments were coagulated and formed in a coagulation bath. The coagulation bath used a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid was controlled at 125 g / L, the concentration of sodium sulfate was 260 g / L, the concentration of zinc sulfate was 6 g / L, and the temperature was controlled at 48°C. The coagulated filaments were washed, desulfurized, oiled, and drawn at a drawing multiple of 2.2 times, and wound to obtain flame-retardant viscose fibers.
[0064] Preparation of flame-retardant core-spun yarn: Aramid fiber with a fineness of 1.5D and a length of 38 mm was selected as the core layer, and the aramid fiber was introduced into the twisting area of the spinning machine through a wire guide device. The flame-retardant polyester fiber and the flame-retardant viscose fiber were fully mixed in a mass ratio of 60:40, and the mixed fibers were sent into the twisting area of the spinning machine for coating and twisting with the core layer fibers. The spindle speed of the spinning machine was controlled at 8500 rpm to obtain the flame-retardant core-spun yarn.
[0065] The flame retardant core-spun yarn prepared in this embodiment was tested for performance, and its breaking strength was 19.0 cN / Tex, the breaking elongation was 12.3%, the limiting oxygen index was 31.0%, the afterflaming time in the vertical burning test was 2.0 s, and the damaged length was 10.5 cm.
[0066] Comparative Example
[0067] Preparation of polyester fiber: Put the polyester chips into a vacuum drying oven and dry them at 125°C for 9 hours. Turn the chips every 2 hours to reduce the moisture content of the chips to 0.01%. Convert the dried polyester chips into polyester fibers through a spinning process. The spinning speed is controlled at 1100m / min and the stretching multiple is set to 4 times, so that the fiber fineness reaches 1.8dtex.
[0068] Preparation of viscose fiber: testing the viscose stock solution, putting the viscose stock solution into a stirring kettle, stirring for 2.5 hours at a stirring speed of 120 rpm, filtering the prepared solution to remove impurities and undissolved particles, extruding the filtered solution through a spinneret to form filaments, the spinneret having an aperture of 0.15 mm and 120 holes, and coagulating the filaments in a coagulation bath, wherein the coagulation bath adopts a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid is controlled at 130 g / L, the concentration of sodium sulfate is 280 g / L, the concentration of zinc sulfate is 8 g / L, and the temperature is controlled at 50°C, washing, desulfurization, oiling, and drawing treatment are performed on the coagulated filaments, the drawing multiple is 2.5 times, and winding is performed to obtain viscose fiber.
[0069] Preparation of core-spun yarn: select ordinary fiber with a fineness of 1.5D and a length of 38 mm as the core layer, introduce the ordinary fiber into the twisting area of the spinning machine through a wire guide device, fully mix the polyester fiber and the viscose fiber in a mass ratio of 60:40, and send the mixed fiber into the twisting area of the spinning machine to be coated and twisted with the core layer fiber. The spindle speed of the spinning machine is controlled at 9000 rpm to obtain the core-spun yarn.
[0070] The core-spun yarn prepared in this comparative example was tested for performance, and its breaking strength was 15.5 cN / Tex, the breaking elongation was 10.5%, the limiting oxygen index was 20.5%, the afterflaming time in the vertical burning test was 5.5 s, and the damaged length was 25 cm.
[0071] Common polyester fiber and common viscose fiber were blended in a mass ratio of 60:40 as the sheath layer, and aramid fiber was used as the core layer to prepare the core-spun yarn. The performance of the core-spun yarn prepared in Example 1, Example 2, Example 3, Example 4, Example 5 and the comparative example was tested. The results are shown in the following table:
[0072]
[0073] As described in the table above, by analyzing the performance test results of Examples 1 to 5 and the comparative example, it can be clearly seen that the significant advantages of the present invention are obvious. In terms of breaking strength, the examples are significantly higher than the comparative example, which indicates that the flame-retardant core-spun yarn prepared by the present invention has better mechanical properties; in terms of elongation at break, the examples are also better than the comparative example, reflecting better flexibility and durability. In terms of the key flame-retardant performance indicator limiting oxygen index, the examples are far superior to the comparative example, showing excellent flame retardant ability; in the vertical burning test, the afterburning time of the examples is greatly shortened, and the damaged length is significantly reduced. The various embodiments of the present invention have excellent performance in mechanical properties and flame retardant properties, which are qualitatively improved compared with the traditional comparative example, proving the effectiveness and advancement of the flame-retardant core-spun yarn and the preparation method thereof proposed in the present invention, and can meet higher requirements for core-spun yarn performance.
[0074] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A flame retardant core-spun yarn, characterized in that: The flame retardant core-spun yarn consists of a core layer and a skin layer, specifically including: The core layer is made of aramid fiber, which is para-aramid, i.e. poly(p-phenylene terephthalamide) fiber, which has extremely high molecular chain regularity and crystallinity, giving it excellent high temperature resistance, and its high strength and high modulus provide inner core support for the core-spun yarn; The skin layer is made of a blend of flame-retardant polyester fiber and flame-retardant viscose fiber; The flame retardant polyester fiber is composed of polyester chips and flame retardants. The polyester chips are polyethylene terephthalate (PET) chips. The added flame retardants include organic phosphorus flame retardants and inorganic flame retardants, namely phosphate compounds and aluminum hydroxide. These flame retardants are uniformly dispersed in the polyester matrix through chemical reactions, and form a heat-insulating and oxygen-isolating protective layer during combustion, thereby preventing the spread of flames. The flame retardant viscose fiber comprises viscose stock solution and flame retardant. The viscose stock solution is obtained by chemically treating natural cellulose. The flame retardant used is the same as that in the flame retardant polyester fiber, including organic and inorganic types.
2. The flame-retardant core-spun yarn according to claim 1, characterized in that: The aramid fiber used in the core layer has a fineness of 1.5D and a fiber length of 38mm. The breaking strength of the aramid fiber is 20cN / Tex and the breaking elongation is 2.5%, which makes the core layer have excellent resistance when subjected to tensile force.
3. The flame-retardant core-spun yarn according to claim 1, characterized in that: The organic phosphorus flame retardant in the skin layer achieves flame retardant effect by promoting charring of polyester and making the carbon layer stable and dense, while the inorganic flame retardant plays a flame retardant role by decomposing, absorbing heat and diluting combustible gas.
4. The flame-retardant core-spun yarn according to claim 3, characterized in that: The mass ratio of polyester chips to flame retardant in the flame retardant polyester fiber is 100:
12. When the addition amount of the flame retardant is 10, the afterburning time of the flame retardant polyester fiber in a vertical combustion test can be shortened to 2s, and the damaged length is reduced to 10cm. When the addition amount reaches 15, the limiting oxygen index is increased to 32%, showing more excellent flame retardant properties.
5. The flame-retardant core-spun yarn according to claim 1, characterized in that: In the flame-retardant viscose fiber, the mass ratio of viscose stock solution to flame retardant is 100:
10. When the amount of flame retardant added is 8, the initial decomposition temperature of the fiber in thermogravimetric analysis increases by 50°C. When the amount of flame retardant added reaches 12, the peak value of heat release rate in cone calorimeter test decreases by 30kW / m 2 , suppressing the intensity of combustion.
6. A method for preparing a flame retardant core-spun yarn, characterized in that: The specific steps of the preparation method are: S1. Preparation of flame retardant polyester fiber: S1.1, Slice drying: Place the polyester slices in a vacuum drying oven for deep drying, using the vacuum environment to remove moisture; S1.2, co-extrusion: add the dried polyester chips and flame retardant into the twin-screw extruder, divide the heating area of the extruder, and under the high temperature and the shearing and mixing action of the twin screws, the polyester chips and the flame retardant are fully blended; S1.3, spinning molding: the prepared flame retardant polyester chips are converted into flame retardant polyester fibers through a spinning process. During the spinning process, the spinning speed is controlled at 1000-1200 m / min, and the stretching multiple is set to 3-5 times, so that the fiber fineness reaches 1.5-2.0 dtex. S2. Preparation of flame retardant viscose fiber: S2.1, stock solution preparation: fully mix the viscose stock solution and the flame retardant, and monitor the temperature and viscosity changes of the solution in real time during the mixing process; S2.2, precision spinning: the prepared mixed solution is filtered to remove impurities and undissolved particles, the filtered solution is extruded through a spinneret to form filaments, the spinneret has an aperture of 0.1-0.2 mm and 80-150 holes, the filaments are coagulated in a coagulation bath, the coagulated filaments are washed, desulfurized, oiled, and stretched with a stretching multiple of 2-3 times, and wound to obtain flame-retardant viscose fibers. S3. Preparation of flame retardant core-spun yarn: S3.1, core layer introduction: select aramid fiber with a fineness of 1.5D and a length of 38mm as the core layer, and introduce the aramid fiber into the twisting area of the spinning machine through the wire guide device; S3.2, skin coating molding: the flame retardant polyester fiber and the flame retardant viscose fiber are fully mixed in a mass ratio of 60:40, and the mixed fibers are fed into the twisting area of the spinning machine to be coated and twisted with the core layer fibers. The spindle speed of the spinning machine is controlled at 8000-10000 rpm to obtain the flame retardant core-spun yarn.
7. A method for preparing a flame-retardant core-spun yarn according to claim 6, characterized in that: In the step S1.1, the polyester chips are placed in a vacuum drying oven and dried at 120-130° C. for 8-10 hours. During this process, the chips are turned over every 2 hours to reduce the water content of the chips to 0.01%.
8. A method for preparing a flame-retardant core-spun yarn according to claim 6, characterized in that: In the step S1.2, the fully dried polyester chips and the flame retardant are added into a twin-screw extruder in a mass ratio of 100:
15. The temperature of each section of the twin-screw extruder is set to: 250°C in zone 1, 260°C in zone 2, 270°C in zone 3, and 280°C in zone 4. During the extrusion process, the screw speed is controlled at 200-300 rpm to allow the polyester chips and the flame retardant to be fully melted and blended, and evenly dispersed to form a polyester melt with flame retardant properties.
9. A method for preparing a flame-retardant core-spun yarn according to claim 6, characterized in that: The S2.1 tests the viscose stock solution, puts the viscose stock solution into a stirring kettle, slowly adds the flame retardant into the viscose stock solution at a mass ratio of 100:12 under a stirring speed of 100-150 rpm, and continues stirring for 2-3 hours to fully dissolve the flame retardant and evenly disperse it in the viscose stock solution.
10. A method for preparing a flame-retardant core-spun yarn according to claim 6, characterized in that: The S2.2 coagulation bath adopts a mixed solution of sulfuric acid, sodium sulfate and zinc sulfate, wherein the concentration of sulfuric acid is controlled at 120-150 g / L, the concentration of sodium sulfate is 250-300 g / L, the concentration of zinc sulfate is 5-10 g / L, and the temperature is controlled at 45-55°C.