Preparation method of alumina-based nanofiber membrane and alumina-based nanofiber membrane

By introducing spinning additives into the alumina-silica composite sol and using conjugated electrospinning technology, combining two-stage calcination and organic impregnation treatment, the problem of insufficient mixing uniformity and strength of alumina-based nanofiber membrane is solved. , the preparation of alumina-based nanofiber membranes for high strength and high temperature use is achieved.

CN118957871AActive Publication Date: 2024-11-15ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO

Patent Information

Application Number
CN202411022127.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

In the existing preparation methods for alumina-based nanofiber films, the alumina-silica composite spinning solution is difficult to mix evenly, the fiber membrane strength and use temperature are insufficient, and the fiber membrane thickness is difficult to accurately control.

Method used

By introducing an aluminum source and a silicon source at the beginning of the reaction, an alumina-silicon composite sol was formed, and after concentration and aging, spinning additives were added. The spinning solution was prepared by conjugated electrospinning technology, followed by drying and two-stage calcination. and organic impregnation to obtain an alumina-based nanofiber membrane.

Benefits of technology

The molecular level uniform mixing of alumina-based nanofiber membrane is achieved, which improves the strength and use temperature of the fiber membrane, and controls the thickness and diameter of the fiber membrane, which enhances its comprehensive use performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957871A_ABST
    Figure CN118957871A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an alumina-based nanofiber membrane and the alumina-based nanofiber membrane, and belongs to the field of inorganic ceramic fibers. Comprising the following steps: mixing an aluminum source, a silicon source, a catalyst and a solvent for reaction to obtain aluminum oxide-silicon oxide composite sol; concentrating and aging the obtained aluminum oxide-silicon oxide composite sol, and then adding a spinning auxiliary agent to obtain a spinning solution; performing conjugate electrostatic spinning on the spinning solution to obtain an alumina-based gel fiber membrane; and carrying out drying, two-stage calcination and organic matter impregnation on the alumina-based gel fiber membrane to obtain the alumina-based nanofiber membrane. An aluminum source and a silicon source are introduced in the initial stage of the reaction, so that a spinning solution can be uniformly mixed at a molecular level; through conjugate electrostatic spinning, the strength of the fiber membrane is improved; through two-stage calcination, the abnormal growth of aluminum oxide grains is avoided; and the machinability is improved through organic matter impregnation. Therefore, the comprehensive use performance of the alumina-based nanofiber membrane is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of inorganic ceramic fibers, and in particular to a method for preparing an alumina-based nanofiber membrane and an alumina-based fiber membrane. Background Art

[0002] With the development of advanced composite materials and their application in the field of high-tech, oxide ceramic fibers are increasingly valued. Compared with ordinary glass fibers or silicon carbide fibers, alumina-based nanofiber membranes have the characteristics of light weight, porosity, low thermal conductivity, high temperature oxidation resistance, and corrosion resistance. They have potential application prospects in high temperature insulation, high temperature filtration, catalyst carriers, etc.

[0003] In the prior art, the preparation method of ceramic fiber membrane mainly uses ceramic fiber as the main raw material, and prepares ceramic fiber membrane through wet forming processes such as pulping, dispersion, and suction filtration. The preparation process is complicated, and the prepared ceramic fiber membrane has a low aluminum oxide content and a relatively coarse fiber diameter. There are also other technologies for preparing alumina fiber membranes, such as preparing alumina fiber membranes using centrifugal spinning and air spinning. By combining centrifugal spinning and air spinning techniques, alumina fibers with a size span from micron to nanometer can be obtained, as well as alumina fiber membranes with uniform structure. The fiber membrane prepared by this method has an irregular appearance and the thickness is difficult to accurately control. At the same time, there is also a sol-gel method combined with electrostatic spinning technology to prepare an alumina fiber membrane with good flexibility, but the fiber membrane prepared by the sol-gel method combined with electrostatic spinning technology has a low use temperature and poor strength. Therefore, how to improve the comprehensive performance of alumina-based nanofiber membranes is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The present application provides a method for preparing an alumina-based nanofiber membrane and an alumina-based fiber membrane to solve the following technical problem: how to improve the comprehensive performance of the alumina-based nanofiber membrane.

[0005] In a first aspect, the present application provides a method for preparing an alumina-based nanofiber membrane, the method comprising:

[0006] The aluminum source, the silicon source, the catalyst and the solvent are mixed and reacted to obtain an aluminum oxide-silicon oxide composite sol;

[0007] The obtained alumina-silicon oxide composite sol is concentrated and aged, and then a spinning aid is added to obtain a spinning solution;

[0008] The spinning solution is subjected to conjugate electrospinning to obtain an alumina-based gel fiber membrane;

[0009] The alumina-based gel fiber membrane is dried, calcined in two stages and impregnated with organic matter to obtain an alumina-based nanofiber membrane.

[0010] Optionally, the aluminum source includes aluminum isopropoxide and aluminum nitrate; the silicon source includes tetraethyl silicate; and the catalyst includes glacial acetic acid.

[0011] Optionally, the Al in the alumina-silicon oxide composite sol 3+ With Si 4+ The molar ratio is (5-20):1.

[0012] Optionally, the addition amount of the spinning aid is 5%-20% of the mass of the spinning solution, and the spinning aid includes one or more of polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone.

[0013] Optionally, the process conditions of the conjugate electrospinning include: double-needle spinning, a spinning solution ejection rate of 0.5 mL / h to 1.5 mL / h, a spinning voltage of 10 KV to 20 KV, and a spinning distance of 10 cm to 20 cm.

[0014] Optionally, the alumina-based gel fiber membrane is dried, calcined in two stages, and impregnated with organic matter to obtain an alumina-based nanofiber membrane, comprising:

[0015] drying the alumina-based gel fiber membrane;

[0016] The dried alumina-based gel fiber membrane is subjected to a first-stage calcination;

[0017] calcining the alumina-based gel fiber membrane after the first-stage calcination in the second stage;

[0018] Cooling the alumina-based gel fiber membrane after the second stage calcination;

[0019] The cooled alumina-based gel fiber membrane is impregnated with organic matter to obtain an alumina-based nanofiber membrane.

[0020] Optionally, the calcination rate of the first stage is 0.5°C / min-2°C / min, the terminal temperature of the first stage calcination is 500°C-800°C, and the holding time of the first stage calcination is 60min-180min; the calcination rate of the second stage is 5°C / min-15°C / min, the terminal temperature of the second stage calcination is 1300°C-1500°C, and the holding time of the second stage calcination is 1min-60min; the terminal temperature of the cooling is room temperature.

[0021] Optionally, the organic matter concentration of the organic matter impregnation is 0.5%-5%, and the organic matter of the organic matter impregnation includes one or more of chitosan, gum arabic and polyvinyl alcohol.

[0022] In a second aspect, the present application provides an alumina-based nanofiber membrane prepared by the method described in any one of the embodiments of the first aspect, wherein the thickness of the alumina-based nanofiber membrane is 10 μm-200 μm, and the fiber diameter of the alumina-based nanofiber membrane is 300 nm-800 nm.

[0023] Optionally, the alumina-based nanofiber membrane satisfies at least one of the following properties: a breaking strength of 5MPa-8MPa, and an operating temperature of 1300°C-1500°C.

[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0025] The present application provides a method for preparing an alumina-based nanofiber membrane, comprising: mixing an aluminum source, a silicon source, a catalyst and a solvent to obtain an alumina-silicon oxide composite sol; concentrating and aging the alumina-silicon oxide composite sol, and then adding a spinning aid to obtain a spinning solution; conjugating the spinning solution to obtain an alumina-based gel fiber membrane; drying, two-stage calcination and organic impregnation of the alumina-based gel fiber membrane to obtain an alumina-based nanofiber membrane. By introducing an aluminum source and a silicon source at the initial stage of the reaction, the spinning solution can be uniformly mixed at the molecular level, solving the problem that the alumina-silicon oxide composite spinning solution is difficult to mix uniformly and is easy to stratify and precipitate; in the electrostatic spinning stage, the alumina nanofibers are staggered by conjugating electrostatic spinning, thereby improving the strength of the fiber membrane; by two-stage calcination, the problem of abnormal growth of the alumina grain size is avoided; by impregnating the fiber membrane with an organic solution, the connection strength between the fibers is enhanced, the strength of the entire fiber membrane is further improved, and its processability is improved. Thereby improving the comprehensive performance of the alumina-based nanofiber membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0028] Figure 1 A schematic diagram of a process for preparing an alumina-based nanofiber membrane provided in an embodiment of the present application;

[0029] Figure 2This is an appearance diagram of the alumina-based nanofiber membrane provided in Example 1 of the present application;

[0030] Figure 3 This is the SEM image of the alumina-based nanofiber membrane provided in Example 1 of the present application. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0033] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0035] Figure 1 A schematic flow chart of a method for preparing an alumina-based nanofiber membrane provided in an embodiment of the present application.

[0036] See also Figure 1 The present application provides a method for preparing an alumina-based nanofiber membrane, the method comprising:

[0037] S1, mixing an aluminum source, a silicon source, a catalyst and a solvent to react to obtain an aluminum oxide-silicon oxide composite sol;

[0038] The present application introduces aluminum source and silicon source at the initial stage of the reaction, so that the spinning solution can be evenly mixed at the molecular level, thereby solving the problem that the aluminum oxide-silicon oxide composite spinning solution is difficult to mix evenly and is easy to stratify and precipitate.

[0039] In some embodiments, the aluminum source includes aluminum isopropoxide and aluminum nitrate; the silicon source includes tetraethyl silicate; and the catalyst includes glacial acetic acid.

[0040] In some embodiments, the Al2O3-SiO2 composite sol 3+ With Si 4+ The molar ratio is (5-20):1.

[0041] Control of Al content in alumina-silicon oxide composite sol 3+ With Si 4+ The molar ratio of Al 3+ :Si 4+ =(5-20):1 is to make the alumina-silicon oxide composite sol spinnable and control the silicon content to inhibit the growth of alumina grains during the later fiber sintering process. The disadvantage of taking a value that is too small is that the silicon content is too high, and the growth of alumina grains cannot be inhibited during the later fiber sintering process. The disadvantage of taking a value that is too large is that the spinnability of the sol deteriorates. For example, Al 3+ With Si 4+ The molar ratio can be 5:1, 8:1, 10:1, 12:1, 15:1, 18:1, 20:1, etc.

[0042] In some embodiments, in the alumina-silicon oxide composite sol, the content of aluminum isopropoxide is 10%-25%, the content of aluminum nitrate is 5%-20%, the content of tetraethyl silicate is 1%-10%, and the content of glacial acetic acid is 1%-5%, by mass fraction.

[0043] The reason for controlling the content of each component in the alumina-silicon oxide composite sol is to reasonably design the chemical composition of the alumina-silicon oxide composite sol, on the one hand, to ensure that the Al in the alumina-silicon oxide composite sol 3+ With Si 4+ On the one hand, the molar ratio meets the preset requirements, and on the other hand, the catalytic effect of glacial acetic acid is guaranteed.

[0044] In some embodiments, the solvent is water and the like.

[0045] S2, concentrating and aging the obtained alumina-silicon oxide composite sol, and then adding a spinning aid to obtain a spinning solution;

[0046] In some embodiments, the addition amount of the spinning aid is 5%-20% of the mass of the spinning solution, and the spinning aid includes one or more of polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone.

[0047] The reason for controlling the addition amount of the spinning aid to 5%-20% is to enable the spinning solution to be electrostatically spun without having too high an organic content that affects the strength of the fiber membrane. If the value is too small, no fiber will come out during the electrostatic spinning process. If the value is too large, the organic matter will volatilize after calcination in the later stage, causing the fiber membrane strength to deteriorate. Exemplarily, the addition amount of the spinning aid is 5%, 7%, 10%, 12%, 15%, 18%, 20%, etc. of the mass of the spinning solution.

[0048] S3, performing conjugate electrospinning on the spinning solution to obtain an alumina-based gel fiber membrane;

[0049] In some embodiments, the process conditions of the conjugate electrospinning include: double-needle spinning, a spinning solution ejection rate of 0.5 mL / h to 1.5 mL / h, a spinning voltage of 10 KV to 20 KV, and a spinning distance of 10 cm to 20 cm.

[0050] The purpose of using double needle spinning is to make the fibers staggered and improve the strength of the fiber film. The reason for controlling the spinning solution ejection rate to 0.5mL / h-1.5mL / h, the spinning voltage to 10KV-20KV, and the spinning distance to 10cm-20cm is to make the fibers ejected evenly. If it is too small, the fiber amount is insufficient and the efficiency is low. If it is too large, droplets will be ejected. Exemplarily, the spinning solution ejection rate can be 0.5mL / h, 0.8mL / h, 1.0mL / h, 1.2mL / h, 1.4mL / h, 1.5mL / h, etc., the spinning voltage can be 10KV, 12KV, 14KV, 16KV, 18KV, 20KV, etc., and the spinning distance can be 10cm, 12cm, 14cm, 16cm, 18cm, 20cm, etc.

[0051] S4, drying, calcining in two stages and impregnating with organic matter the alumina-based gel fiber membrane to obtain an alumina-based nanofiber membrane.

[0052] In some embodiments, the step of drying, two-stage calcining and organic impregnation of the alumina-based gel fiber membrane to obtain an alumina-based nanofiber membrane comprises:

[0053] drying the alumina-based gel fiber membrane;

[0054] The dried alumina-based gel fiber membrane is subjected to a first-stage calcination;

[0055] calcining the alumina-based gel fiber membrane after the first-stage calcination in the second stage;

[0056] Cooling the alumina-based gel fiber membrane after the second stage calcination;

[0057] The cooled alumina-based gel fiber membrane is impregnated with organic matter to obtain an alumina-based nanofiber membrane.

[0058] The present application can solve the problem of abnormal growth of alumina grain size through two-stage calcination.

[0059] In some embodiments, the calcination rate of the first stage is 0.5°C / min-2°C / min, the terminal temperature of the first stage calcination is 500°C-800°C, and the holding time of the first stage calcination is 60min-180min; the calcination rate of the second stage is 5°C / min-15°C / min, the terminal temperature of the second stage calcination is 1300°C-1500°C, and the holding time of the second stage calcination is 1min-60min; the terminal temperature of the cooling is room temperature.

[0060] Control the heating rate of the first stage calcination treatment to ensure that the fiber does not crack during the removal of free water and crystal water. If the heating rate of the first stage calcination treatment is too high, the water may be removed too quickly and the fiber may crack; if the heating rate of the first stage calcination treatment is too low, the sintering cycle may be too long. Exemplarily, the rate of the first stage calcination can be 0.5°C / min, 0.8°C / min, 1°C / min, 1.2°C / min, 1.5°C / min, 1.8°C / min, 2°C / min, etc., the terminal temperature of the first stage calcination can be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and the holding time of the first stage calcination can be 60min, 70min, 80min, 90min, 100min, 120min, 140min, 160min, 180min, etc.

[0061] The heating rate of the second stage calcination treatment is controlled to effectively achieve the sintering purpose while inhibiting the growth of grains to make the grain size small. If the heating rate of the second stage calcination treatment is too high, the fiber may not be sintered in time and have low strength; if the heating rate of the second stage calcination treatment is too low, the grain size may grow; the temperature of the second stage calcination treatment is controlled to ensure that the alumina fiber is sintered densely and the grain size does not grow, so that the grain size is small. Exemplarily, the calcination rate of the second stage can be 5°C / min, 7°C / min, 9°C / min, 10°C / min, 12°C / min, 14°C / min, 15°C / min, etc., the endpoint temperature of the second stage calcination can be 1300°C, 1320°C, 1350°C, 1380°C, 1400°C, 1450°C, 1480°C, 1500°C, etc., and the holding time of the second stage calcination can be 1min, 10min, 20min, 30min, 40min, 50min, 60min, etc.

[0062] In some embodiments, the organic matter concentration of the organic matter impregnation is 0.5%-5%, and the organic matter of the organic matter impregnation includes one or more of chitosan, gum arabic and polyvinyl alcohol.

[0063] The reason for controlling the organic matter concentration to 0.5%-5% is to improve the strength of the alumina-based nanofiber membrane. If the value is too low, it will not improve the strength, and if the value is too high, it will reduce the flexibility of the fiber membrane. Exemplarily, the organic matter concentration of the organic matter impregnation can be 0.5%, 1%, 2%, 3%, 4%, 5%, etc.

[0064] Based on a general inventive concept, the present application provides an alumina-based nanofiber membrane prepared by the method described in any one of the above embodiments, wherein the thickness of the alumina-based nanofiber membrane is 10μm-200μm, and the fiber diameter of the alumina-based nanofiber membrane is 300nm-800nm.

[0065] In some embodiments, the alumina-based nanofiber membrane satisfies at least one of the following properties: a breaking strength of 5 MPa-8 MPa, and an operating temperature of 1300°C-1500°C.

[0066] The present application introduces aluminum source and silicon source at the initial stage of the reaction, which can make the spinning solution evenly mixed at the molecular level, solving the problem that the aluminum oxide-silicon oxide composite spinning solution is difficult to mix evenly and easy to stratify and precipitate; in the electrostatic spinning stage, the aluminum oxide nanofibers are staggered by conjugated electrostatic spinning, which improves the strength of the fiber membrane; through two-stage calcination, the problem of abnormal growth of the aluminum oxide grain size is avoided; by using an organic solution to impregnate the fiber membrane, the connection strength between the fibers is enhanced, the strength of the entire fiber membrane is further improved, and its processability is improved. Thereby improving the comprehensive performance of the aluminum oxide-based nanofiber membrane. Exemplarily, the thickness of the aluminum oxide-based nanofiber membrane can be 10μm, 30μm, 50μm, 80μm, 100μm, 120μm, 150μm, 200μm, etc., and the fiber diameter of the aluminum oxide-based nanofiber membrane can be 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, etc. The breaking strength of the alumina-based nanofiber membrane can be 5MPa, 5.5MPa, 6MPa, 6.5MPa, 7MPa, 7.5MPa, 8MPa, etc., and the operating temperature can be 1300℃, 1320℃, 1350℃, 1380℃, 1400℃, 1450℃, 1480℃, 1500℃, etc.

[0067] The alumina-based nanofiber membrane is prepared based on the above-mentioned method for preparing the alumina-based nanofiber membrane. The specific steps of the method for preparing the alumina-based nanofiber membrane can refer to the above-mentioned embodiment. Since the alumina-based nanofiber membrane adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.

[0068] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0069] Example 1

[0070] This embodiment provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0071] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 10.0g of aluminum nitrate nonahydrate, 12.0g of aluminum isopropoxide, 2.0g of glacial acetic acid, and 1.5g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0072] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl alcohol thereto to obtain a spinning solution; wherein the amount of polyvinyl alcohol added is 10% of the mass of the spinning solution;

[0073] S31, adding the spinning solution into the electrospinning equipment to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 1.0 mL / h, the spinning voltage is 15 KV, the spinning distance is 12 cm, and an alumina-based gel fiber membrane is obtained;

[0074] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 600°C at 1°C / min and keep it warm for 60 minutes. The second stage of calcination is to quickly increase the temperature to 1300°C at 10°C / min and keep it warm for 5 minutes. The membrane is then cooled to room temperature and then immersed in organic matter in a 1% polyvinyl alcohol solution and dried to obtain an alumina-based nanofiber membrane.

[0075] Example 2

[0076] This embodiment provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0077] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 8.0g of aluminum nitrate nonahydrate, 13.0g of aluminum isopropoxide, 3.0g of glacial acetic acid, and 3.0g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0078] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl pyrrolidone thereto to obtain a spinning solution; wherein the amount of polyvinyl pyrrolidone added is 15% of the mass of the spinning solution;

[0079] S31, adding the spinning solution to an electrospinning device to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 0.5 mL / h, the spinning voltage is 10 KV, the spinning distance is 15 cm, and an alumina-based gel fiber membrane is obtained;

[0080] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 500°C at a rate of 0.5°C / min and keep it warm for 120 minutes. The second stage of calcination is to quickly increase the temperature to 1400°C at a rate of 5°C / min and keep it warm for 1 minute. The membrane is then cooled to room temperature and then immersed in a 3% chitosan solution for organic matter and dried to obtain an alumina-based nanofiber membrane.

[0081] Example 3

[0082] This embodiment provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0083] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 7.0g of aluminum nitrate nonahydrate, 12.0g of aluminum isopropoxide, 1.5g of glacial acetic acid, and 1.0g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0084] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyethylene oxide thereto to obtain a spinning solution; wherein the amount of polyethylene oxide added is 20% of the mass of the spinning solution;

[0085] S31, adding the spinning solution to an electrospinning device to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 1.5 mL / h, the spinning voltage is 20 KV, the spinning distance is 20 cm, and an alumina-based gel fiber membrane is obtained;

[0086] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 700°C at 2°C / min and keep it warm for 60 minutes. The second stage of calcination is to quickly increase the temperature to 1500°C at 15°C / min and keep it warm for 5 minutes. The membrane is then cooled to room temperature and then immersed in a 5% gum arabic solution for organic matter impregnation and dried to obtain an alumina-based nanofiber membrane.

[0087] Example 4

[0088] This embodiment provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0089] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 6.5g of aluminum nitrate nonahydrate, 11.5g of aluminum isopropoxide, 1.5g of glacial acetic acid, and 2.0g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0090] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl pyrrolidone thereto to obtain a spinning solution; wherein the amount of polyvinyl pyrrolidone added is 10% of the mass of the spinning solution;

[0091] S31, adding the spinning solution into the electrospinning equipment to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 0.8mL / h, the spinning voltage is 12KV, the spinning distance is 15cm, and an alumina-based gel fiber membrane is obtained;

[0092] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to heat up to 600°C at 1°C / min and keep it warm for 30 minutes. The second stage of calcination is to quickly heat up to 1300°C at 10°C / min and keep it warm for 30 minutes. The membrane is then cooled to room temperature and then immersed in organic matter in a 0.5% polyvinyl alcohol solution and dried to obtain an alumina-based nanofiber membrane.

[0093] Example 5

[0094] This embodiment provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0095] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 6.0g of aluminum nitrate nonahydrate, 8.0g of aluminum isopropoxide, 1.5g of glacial acetic acid, and 0.6g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0096] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl alcohol thereto to obtain a spinning solution; wherein the amount of polyvinyl alcohol added is 5% of the mass of the spinning solution;

[0097] S31, adding the spinning solution into the electrospinning equipment to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 1.0 mL / h, the spinning voltage is 18 KV, the spinning distance is 20 cm, and an alumina-based gel fiber membrane is obtained;

[0098] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 800°C at a rate of 1.5°C / min and keep it warm for 60 minutes. The second stage of calcination is to quickly increase the temperature to 1300°C at a rate of 5°C / min and keep it warm for 60 minutes. The membrane is then cooled to room temperature and then immersed in a 2% gum arabic solution for organic matter and dried to obtain an alumina-based nanofiber membrane.

[0099] Comparative Example 1

[0100] This comparative example provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0101] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 8.0g of aluminum nitrate nonahydrate, 12.0g of aluminum isopropoxide, 2.0g of glacial acetic acid, and 2.0g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0102] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl alcohol thereto to obtain a spinning solution; wherein the amount of polyvinyl alcohol added is 15% of the mass of the spinning solution;

[0103] S31, adding the spinning solution to an electrospinning device to perform conjugate electrospinning, the spinning process conditions are: single needle spinning, the spinning solution ejection rate is 0.5 mL / h, the spinning voltage is 15 KV, the spinning distance is 15 cm, and an alumina-based gel fiber membrane is obtained;

[0104] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 600°C at 1°C / min and keep it warm for 120 minutes. The second stage of calcination is to quickly increase the temperature to 1400°C at 10°C / min and keep it warm for 10 minutes. The membrane is then cooled to room temperature and then immersed in a 1% gum arabic solution for organic matter and dried to obtain an alumina-based nanofiber membrane.

[0105] Comparative Example 2

[0106] This comparative example provides a method for preparing an alumina-based nanofiber membrane, comprising the following steps:

[0107] S11, add 50g of deionized water into a 1L three-necked round-bottom flask, add 6.0g of aluminum nitrate nonahydrate, 8.0g of aluminum isopropoxide, 1.5g of glacial acetic acid, and 0.6g of tetraethyl silicate in sequence, stir evenly, and then perform a mixing reaction to obtain an aluminum oxide-silicon oxide composite sol;

[0108] S21, concentrating and aging the alumina-silicon oxide composite sol, and then adding polyvinyl pyrrolidone thereto to obtain a spinning solution; wherein the amount of polyvinyl pyrrolidone added is 10% of the mass of the spinning solution;

[0109] S31, adding the spinning solution into the electrospinning equipment to perform conjugate electrospinning, the spinning process conditions are: double needle spinning, the spinning solution ejection rate is 0.8mL / h, the spinning voltage is 10KV, the spinning distance is 12cm, and an alumina-based gel fiber membrane is obtained;

[0110] S41. The alumina-based gel fiber membrane is calcined in two stages. The first stage of calcination is to increase the temperature to 500°C at a rate of 0.5°C / min and keep it warm for 30 minutes. The second stage of calcination is to quickly increase the temperature to 1300°C at a rate of 5°C / min and keep it warm for 30 minutes. The membrane is then cooled to room temperature and then immersed in organic matter in a 0.1% polyvinyl alcohol solution and dried to obtain an alumina-based nanofiber membrane.

[0111] Related experiments and effect data:

[0112] The performance of the alumina-based nanofiber membranes provided in Examples 1-5 and Comparative Examples 1-2 was characterized, and the results are shown in the following table.

[0113] Table 1 Performance of the alumina-based nanofiber membranes prepared in Examples and Comparative Examples

[0114]

[0115]

[0116] It can be seen from the above table that the alumina-based nanofiber membrane prepared by the method provided in the embodiment of the present application has controllable thickness and fiber diameter, and has high strength and operating temperature.

[0117] Observe the alumina-based nanofiber membrane provided in Example 1. Figure 2 The figure shows the appearance of the alumina-based nanofiber membrane prepared in Example 1. Figure 2 It can be seen that the alumina-based nanofiber membrane has a smooth appearance and good flexibility.

[0118] The alumina-based nanofiber membrane provided in Example 1 was subjected to microstructural testing, and the results were as follows: Figure 3 The SEM image of the alumina-based nanofiber membrane prepared in Example 1 is shown in FIG. Figure 3 It can be seen that the fibers are staggered and the fiber diameter is about 500 nanometers.

[0119] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0120] (1) In the embodiment of the present invention, the method for preparing the alumina fiber membrane provided solves the problems of low operating temperature, poor strength and inability to accurately control the thickness of the alumina fiber membrane in the prior art.

[0121] (2) In the embodiment of the present invention, the obtained alumina-based nanofiber membrane has a thickness of 10 μm-200 μm, a fiber diameter of 300 nm-800 nm, a breaking strength of 5 MPa-8 MPa, and an operating temperature of 1200° C.-1400° C. The fiber membrane has good flexibility, is not easy to break, has strong processability, and can be used as a high-temperature insulation material or a high-temperature filtration material.

[0122] (3) In the embodiments of the present invention, the obtained alumina-based nanofiber membrane has the characteristics of light weight, porosity, low thermal conductivity, high temperature oxidation resistance, and corrosion resistance, and has potential application prospects in high temperature insulation, high temperature filtration, catalyst carrier, etc.

[0123] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing an alumina-based nanofiber membrane, characterized in that: The method comprises: The aluminum source, the silicon source, the catalyst and the solvent are mixed and reacted to obtain an aluminum oxide-silicon oxide composite sol; The obtained alumina-silicon oxide composite sol is concentrated and aged, and then a spinning aid is added to obtain a spinning solution; The spinning solution is subjected to conjugate electrospinning to obtain an alumina-based gel fiber membrane; The alumina-based gel fiber membrane is dried, calcined in two stages and impregnated with organic matter to obtain an alumina-based nanofiber membrane.

2. The method according to claim 1, characterized in that: The aluminum source includes aluminum isopropoxide and aluminum nitrate; the silicon source includes tetraethyl silicate; and the catalyst includes glacial acetic acid.

3. The method according to claim 1, characterized in that The Al2O3-SiO2 composite sol 3+ With Si 4+ The molar ratio is (5-20):

1.

4. The method according to claim 1, characterized in that: The addition amount of the spinning aid is 5%-20% of the mass of the spinning solution, and the spinning aid includes one or more of polyethylene oxide, polyvinyl alcohol and polyvinyl pyrrolidone.

5. The method according to claim 1, characterized in that The process conditions of the conjugate electrospinning include: double needle spinning, a spinning solution ejection rate of 0.5 mL / h to 1.5 mL / h, a spinning voltage of 10 KV to 20 KV, and a spinning distance of 10 cm to 20 cm.

6. The method according to claim 1, characterized in that The alumina-based gel fiber membrane is dried, calcined in two stages, and impregnated with organic matter to obtain an alumina-based nanofiber membrane, comprising: drying the alumina-based gel fiber membrane; The dried alumina-based gel fiber membrane is subjected to a first-stage calcination; calcining the alumina-based gel fiber membrane after the first-stage calcination in the second stage; Cooling the alumina-based gel fiber membrane after the second stage calcination; The cooled alumina-based gel fiber membrane is impregnated with organic matter to obtain an alumina-based nanofiber membrane.

7. The method according to claim 1, characterized in that The calcination rate of the first stage is 0.5°C / min-2°C / min, the terminal temperature of the first stage calcination is 500°C-800°C, and the holding time of the first stage calcination is 60min-180min; the calcination rate of the second stage is 5°C / min-15°C / min, the terminal temperature of the second stage calcination is 1300°C-1500°C, and the holding time of the second stage calcination is 1min-60min; the terminal temperature of the cooling is room temperature.

8. The method according to claim 7, characterized in that The organic matter concentration of the organic matter impregnation is 0.5%-5%, and the organic matter impregnation includes one or more of chitosan, gum arabic and polyvinyl alcohol.

9. An alumina-based nanofiber membrane prepared by the method according to any one of claims 1 to 8, characterized in that: The thickness of the alumina-based nanofiber membrane is 10 μm-200 μm, and the fiber diameter of the alumina-based nanofiber membrane is 300 nm-800 nm.

10. The alumina-based nanofiber membrane according to claim 9, characterized in that: The alumina-based nanofiber membrane meets at least one of the following properties: a breaking strength of 5MPa-8MPa and an operating temperature of 1300°C-1500°C.

Citation Information

Patent Citations

  • Method used for preparing ultra-fine aluminium oxide fiber by electrospinning of pseudo-boehmite sol

    CN103469366A

  • High temperature resistance and corrosion resistance inorganic filtration fiber membrane and preparation method thereof

    CN107604537A

  • Aluminum oxide ceramic filament and preparation method for sol-gel spinning thereof

    CN110041055A

  • Polyimide reinforced and toughened silicon dioxide nanofiber membrane and preparation method thereof

    CN114164666A

  • Porous mullite nanofiber-based flocculus material with vertical orientation structure and preparation method of porous mullite nanofiber-based flocculus material

    CN114455846A

Cited By

  • Preparation method of ceramic nanofiber compounded with silicon dioxide and aluminum oxide

    CN120174511A