Fiber cloth material with magnetic composite photocatalyst and preparation method thereof

By forming a copper or silver dispersed magnetic composite photocatalyst on the fiber cloth, the problem of insufficient visible light absorption capacity of existing photocatalytic materials is solved, realizing green production with high efficiency photocatalytic activity and easy recycling, which is suitable for self-cleaning fiber cloth.

CN118957977APending Publication Date: 2024-11-15GUANGZHOU GUANGYUCHAO MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005465.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing photocatalytic materials have insufficient visible light absorption capacity and fast recombination rate of photogenerated holes and electron pairs, which limits their application in real life. In addition, traditional methods have problems such as low content of composite photocatalysts, high production costs, and strict environmental requirements.

Method used

Using a roughened fiber cloth as a substrate, Fe(OH)2 is generated through the coordination of hydrophilic groups with ferrous ions. Subsequently, it reacts with copper or silver ammonia solution to form a magnetic composite photocatalyst in which copper or silver is dispersed in iron oxide, forming nano-sized particles that promote the separation and transport of photogenerated electron-hole pairs.

Benefits of technology

It improves the absorption efficiency of photocatalysts for visible light, enhances photocatalytic activity, and achieves significant degradation and antibacterial effects on organic dyes and heavy metals. The material is easy to recycle and meets the requirements of green chemical production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957977A_ABST
    Figure CN118957977A_ABST
Patent Text Reader

Abstract

The invention discloses a fiber cloth material with a magnetic composite photocatalyst and a preparation method thereof.The fiber cloth material is characterized in that fiber cloth with the roughened surface and modified with a large number of hydrophilic groups is adopted, and the surface of the fiber cloth is modified with a large number of ferrous ions through the coordination effect of the hydrophilic groups and the ferrous ions; ferrous ions on the surface of the fiber cloth are converted into Fe (OH) 2; then Fe (OH) 2 reacts with a copper ammonia solution or Fe (OH) 2 reacts with a silver ammonia solution, the magnetic composite photocatalyst is generated on the surface of the fiber cloth, and the preparation method is simple. The magnetic composite photocatalyst comprises ferroferric oxide and copper or / and silver, the copper or / and silver is / are dispersed and distributed in the ferroferric oxide, visible light can be efficiently absorbed, electron-hole pairs can be generated, the electron-hole pairs can be efficiently separated, generated active free radicals have an obvious degradation effect on organic dye and heavy metal, meanwhile, the antibacterial effect is obvious, and the magnetic composite photocatalyst has a good application prospect. The excellent photocatalytic performance is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials, and in particular to a fiber cloth material with a magnetic composite photocatalyst and a preparation method thereof. Background Art

[0002] Photocatalytic technology has the advantages of being green, clean, fast, and highly selective, and has been widely used in wastewater treatment, redox catalysis, and other fields. Photocatalytic technology refers to the process in which the electrons of photocatalytic materials jump from the valence band to the conduction band under light conditions to generate photogenerated electrons and photogenerated holes. When photogenerated electrons and photogenerated holes encounter water and oxygen, they can generate highly chemically active free radicals such as hydroxyl radicals and superoxide radicals. The active free radicals can decompose large organic molecules into small organic molecules and inorganic substances, thereby achieving the effect of degrading organic matter or inactivating microorganisms.

[0003] At present, photocatalytic materials are mainly semiconductor materials, among which oxide semiconductor materials have attracted much attention due to their easy preparation and low cost, such as titanium dioxide and zinc oxide. However, oxide semiconductors have poor visible light absorption, severe photochemical corrosion, and fast recombination of photogenerated hole-electron pairs, which greatly limits their application in real life. Therefore, the design and development of composite oxide semiconductor materials has become a new research hotspot.

[0004] For example, the Chinese patent with the announcement number CN113104995A uses the sol-gel method to prepare a composite photocatalyst of modified magnetic powder and titanium dioxide, and then loads the photocatalyst on a polyurethane sponge by spraying or dipping. After the obtained magnetic polyurethane sponge is inoculated with active microorganisms, it can degrade a variety of polluted wastewater under ultraviolet irradiation. However, in this method, the composite photocatalyst content in the magnetic sponge is low, and the titanium dioxide content in the composite photocatalyst is high, and the absorption of visible light is extremely weak, and the catalytic degradation ability under sunlight is limited.

[0005] For example, the Chinese patent with announcement number CN111834128A prepares a silver-iron oxide composite material by thermally decomposing an organic silver salt and an organic iron salt at a high temperature, and then mixes and disperses the composite material with n-hexane and PU glue to prepare a suspension slurry. The slurry is dripped onto the surface of a conductive substrate and dried and thermally decomposed to prepare a silver-iron oxide composite structure thin film electrode with higher photoelectric conversion capacity and lower production cost. However, each production requires a large amount of organic solvent and the mass of the target product is at the milligram level, which does not meet the requirements of modern green chemical industry production.

[0006] For example, in announcement number CN110124636A, magnetic composite quantum dots were mixed with a polymer mixed solution and a nanoscale magnetic composite fiber material was successfully prepared by using an electrospinning method. The material has the characteristics of large specific surface area and many active sites, and can process a variety of heavy metals and non-metallic pollutants under visible light. However, the electrospinning technology has a slow production rate, high requirements on environmental temperature and humidity, and poor secondary processing capabilities of the nanofibers.

[0007] In view of this, the present invention proposes a fiber cloth material with a magnetic composite photocatalyst and a preparation method thereof to solve the above problems. Summary of the invention

[0008] In order to overcome the shortcomings of the above-mentioned technology, the present invention provides a fiber cloth material with a magnetic composite photocatalyst, which has good visible light absorption ability, and the generated active free radicals have obvious degradation effects on organic dyes and heavy metals, and at the same time have obvious antibacterial effects and excellent photocatalytic properties.

[0009] To achieve the above-mentioned purpose, the present invention provides a fiber cloth material with a magnetic composite photocatalyst, including a fiber cloth with a roughened surface, wherein the surface of the roughened fiber cloth is loaded with a magnetic composite photocatalyst, and the magnetic composite photocatalyst includes ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

[0010] Preferably, the mass fraction of ferrosoferric oxide in the magnetic composite photocatalyst is greater than the mass fraction of copper and / or silver.

[0011] Preferably, the copper and / or silver are dispersed in ferroferric oxide to form nano-scale magnetic composite photocatalytic particles.

[0012] To achieve the above-mentioned purpose, the present invention further provides a method for preparing a magnetic composite fiber cloth visible light catalytic material, which uses a fiber cloth with a roughened surface and modified with a large number of hydrophilic groups, and through the coordination effect between the hydrophilic groups and ferrous ions, the surface of the fiber cloth is modified with a large number of ferrous ions; the ferrous ions on the surface of the fiber cloth are then converted into Fe(OH)2; then, Fe(OH)2 reacts with a copper ammonia solution, or Fe(OH)2 reacts with a silver ammonia solution, to generate a magnetic composite photocatalyst on the surface of the fiber cloth, wherein the magnetic composite photocatalyst includes ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

[0013] Preferably, the method for preparing a fiber cloth material having a magnetic composite photocatalyst comprises the following steps:

[0014] Step 1: Put the clean fiber cloth into an aqueous solution containing a strong oxidant to roughen the surface of the fiber cloth; then freeze-dry the fiber cloth with the roughened surface to obtain a fiber cloth with a large number of hydrophilic groups on the surface;

[0015] Step 2: Add deionized water and anionic surfactant into the reactor, then add fiber cloth containing a large number of hydrophilic groups, heat in a water bath and stir rapidly;

[0016] Step 3: Adding a ferrous salt aqueous solution into the reactor, the ferrous ions coordinate with the hydrophilic groups of the fiber cloth, so that the surface of the fiber cloth contains a large amount of ferrous ions;

[0017] Step 4: Slowly add ammonia water into the reactor, and the ferrous ions on the surface of the fiber cloth will generate flocculent Fe(OH)2 in an alkaline environment;

[0018] Step 5: slowly dripping a copper ammonia solution or a silver ammonia solution into the reactor as an oxidant to react with the flocculent Fe(OH)2 on the surface of the fiber cloth to generate a fiber cloth material with a magnetic composite photocatalyst;

[0019] Step 6: Magnetic absorption collects the fiber cloth material with magnetic composite photocatalyst in step 5, and washes and dries it;

[0020] In step 3, step 4 and step 5, the reactor is in an oxygen-free state.

[0021] Preferably, the preparation of the clean fiber cloth comprises the following steps: using NaOH solution to decompose the grease on the surface of the fiber cloth, so that the grease is decomposed into small molecular organic matter; then washing the fiber cloth with acetone to wash away the small molecular organic matter on the surface of the fiber cloth; and finally washing away other impurities on the fiber cloth with deionized water and / or ethanol.

[0022] Preferably, in the step 1, a strong oxidant reacts with the fiber cloth under heating conditions at 60-80° C. in a water bath; the strong oxidant is a mixed solution of nitric acid and sulfuric acid or a hydrogen peroxide solution.

[0023] Preferably, in the step 1, the surface roughened fiber cloth is frozen at a temperature of -60 to -30°C and the freezing time is 10 to 14 hours.

[0024] Preferably, in step 4, ammonia water is slowly added dropwise to the reactor and stirred rapidly, and after the addition of ammonia water is completed, the ammonia water continues to react with the ferrous ions on the surface of the fiber cloth for a period of time.

[0025] Preferably, in step 5, the pH in the reactor is ≥10, the reaction temperature is 50-80° C., and after the copper ammonia solution or the silver ammonia solution is added dropwise, the reaction is continued at the temperature for a period of time.

[0026] Preferably, in step 5, after the copper ammonia solution or silver ammonia solution is added dropwise, hydrogen peroxide, hypochlorite or persulfate may be added as an oxidant, and the reaction is continued at the temperature for a period of time.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. Compared with the composite photocatalyst with core-shell structure in the prior art, the magnetic composite photocatalyst of the present invention is a dispersed structure, copper and / or silver are dispersed in ferroferric oxide, the contact area between ferroferric oxide and copper / silver is larger, and the interaction between silver / copper and ferroferric oxide can promote the separation and transmission of photogenerated electron-hole pairs, thereby improving the photocatalytic activity of the composite material. Moreover, copper and silver can broaden the light absorption range of the composite photocatalyst, improve its absorption efficiency of visible light, and thus improve the photocatalytic efficiency.

[0029] 2. The magnetic composite photocatalytic particles of the present invention are nanometer-sized, that is, silver, copper, and ferroferric oxide are all nanometer-sized, with a large specific surface area, thereby increasing the contact area between silver / copper and ferroferric oxide. Moreover, since the bandgap width of ferroferric oxide is within the bandgap width range of inorganic semiconductors, silver / copper and ferroferric oxide form a Schottky junction structure, that is, a built-in potential difference is formed on the contact surface between silver / copper and ferroferric oxide. The built-in potential difference can transfer electrons on ferroferric oxide to silver / copper, thereby effectively separating photogenerated electron-hole pairs, and further improving the photocatalytic activity of the composite material.

[0030] 3. The present invention uses fiber cloth as the substrate, which is cheap, and the fiber cloth has a roughened surface, a large specific surface area and many depressions, which can provide attachment points for the deposition of the magnetic composite photocatalyst.

[0031] 4. After the fiber cloth material of the present invention is used industrially to photocatalytically degrade wastewater, the fiber cloth material and waste liquid can be quickly separated by magnetic attraction, making the fiber cloth material easier to recycle and reuse. At the same time, under the illumination of daily life, the composite photocatalytic fiber has silver / copper, and the photogenerated holes and photogenerated electrons with strong oxidizing properties can clean stains and inhibit the growth of microorganisms on clothing fabrics. The ferroferric oxide, copper, and silver on the surface of the composite fiber are not toxic to the human body, so it has potential application value in self-cleaning and wash-free fiber cloth.

[0032] 5. In the process of preparing the fiber cloth material with magnetic composite photocatalyst, the present invention firstly reacts the fiber cloth with a strong oxidant to roughen the surface of the fiber cloth, increase the concave position for attaching the magnetic composite photocatalyst, and then freeze-dry the roughened surface fiber cloth, so that the fiber cloth is modified with a large number of hydrophilic groups, and the operation is simple. The hydrophilic group coordinates with the ferrous ions, so that a large number of ferrous ions are stably modified on the surface of the fiber cloth. Then the ferrous ions generate flocculent Fe(OH)2 in an alkaline environment. When heated in a water bath, copper / silver ammonia solution is added, Fe(OH)2 is slowly oxidized to Fe3O4, and the copper / silver ammonia ions are reduced to copper / silver. The copper / silver generated by the reaction can be dispersed with Fe3O4, so that copper / silver and Fe3O4 are fully in contact. At the same time, Fe3O4 and copper / silver hinder the continuity of the growth of the two crystals, so that the magnetic composite photocatalyst is a nano-scale particle. The magnetic composite photocatalyst has a quantum size effect, resulting in the formation of a Schottky junction structure between silver / copper and ferroferric oxide.

[0033] 6. The method for preparing the fiber cloth material with magnetic composite photocatalyst of the present invention is simple, the preparation cycle is short, no highly toxic organic solvents are used, the reaction conditions are mild, and it meets the requirements of modern green chemical production. In addition, the fiber cloth is used as a catalyst material substrate and is inexpensive. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The XRD test analysis diagrams of Examples 1 to 3 and Comparative Example 1 of the present invention are shown in FIG.

[0035] Figure 2 The degradation of Congo red dye by Examples 1 to 3 and Comparative Example 1 of the present invention is tC t / C o picture;

[0036] Figure 3 The degradation rate of Cr(VI) in Examples 1 to 3 and Comparative Example 1 is t / C o picture;

[0037] Figure 4 It is the electrochemical impedance analysis diagram of Examples 1 to 3 of the present invention and Comparative Example 1;

[0038] Figure 5 It is the antibacterial test diagram of Examples 1 to 3 of the present invention and Comparative Example 1;

[0039] Figure 6 This is a state diagram of the fiber cloth of the present invention after the surface is roughened;

[0040] Figure 7 This is a state diagram of the fiber cloth material with magnetic composite photocatalyst before cleaning;

[0041] Figure 8 This is a diagram of the state of the fiber cloth material with magnetic composite photocatalyst after cleaning;

[0042] The implementation, functional features and advantages of the present invention will be further described in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0043] The features of the present invention and other related features are further described in detail below through embodiments to facilitate understanding by those skilled in the art:

[0044] An embodiment of the present invention provides a fiber cloth material with a magnetic composite photocatalyst, including a fiber cloth with a roughened surface, wherein the surface of the roughened fiber cloth is loaded with a composite photocatalyst, and the magnetic composite photocatalyst includes ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

[0045] In some embodiments, the mass fraction of ferrosoferric oxide in the magnetic composite photocatalyst is greater than the mass fraction of copper and / or silver.

[0046] In some embodiments, the copper and / or silver are dispersed in ferroferric oxide to form nano-scale magnetic composite photocatalytic particles.

[0047] An embodiment of the present invention also provides a method for preparing a magnetic composite fiber cloth visible light catalytic material, which uses a fiber cloth with a roughened surface and modified with a large number of hydrophilic groups, and through the coordination effect between the hydrophilic groups and ferrous ions, the surface of the fiber cloth is modified with a large number of ferrous ions; the ferrous ions on the surface of the fiber cloth are then converted into Fe(OH)2; then, a magnetic composite photocatalyst is generated on the surface of the fiber cloth by reacting Fe(OH)2 with a copper ammonia solution, or Fe(OH)2 with a silver ammonia solution, wherein the magnetic composite photocatalyst includes ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

[0048] In some embodiments, the method for preparing a fiber cloth material having a magnetic composite photocatalyst comprises the following steps:

[0049] Step 1: Place the clean fiber cloth in an aqueous solution containing a strong oxidant to roughen the surface of the fiber cloth, such as Figure 6 As shown, the roughened fiber cloth increases the concave positions for attaching the magnetic composite photocatalyst. The roughened fiber cloth is then freeze-dried to obtain a fiber cloth having a large number of hydrophilic groups on the surface. The hydrophilic groups include hydroxyl groups and carboxyl groups.

[0050] Step 2: Add deionized water and anionic surfactant to the reactor, then add fiber cloth containing a large number of hydrophilic groups, heat in a water bath and stir rapidly. The anionic surfactant cooperates with the hydrophilic groups of the fiber cloth to fully wet the fiber cloth, which is conducive to the subsequent reaction between the fiber cloth and the solution.

[0051] Step 3: Adding ferrous salt aqueous solution into the reactor, the ferrous ions coordinate with the hydrophilic groups of the fiber cloth, so that the surface of the fiber cloth contains a large amount of ferrous ions.

[0052] Step 4: Slowly add ammonia water into the reactor, and the ferrous ions on the surface of the fiber cloth will generate flocculent Fe(OH)2 in an alkaline environment.

[0053] Step 5: Slowly add copper / silver ammonia solution to the reactor to react with the flocculent Fe(OH)2 on the surface of the fiber cloth to generate a fiber cloth material with a magnetic composite photocatalyst.

[0054] Step 6: Magnetic absorption collects the fiber cloth material with magnetic composite photocatalyst in step 5, and washes and dries it. Figures 7-8 As shown, after washing and drying, the fiber cloth does not obviously fall off the magnetic composite photocatalyst, indicating that the preparation method of the present invention can make the magnetic composite photocatalyst firmly bonded to the fiber cloth. Moreover, the magnetic composite photocatalyst is a 20-600nm particle.

[0055] In step 3, step 4 and step 5, the reactor is in an oxygen-free state to prevent ferrous ions and Fe(OH)2 from being oxidized prematurely and affecting the structure of the magnetic composite photocatalyst.

[0056] In some embodiments, in step one, the preparation of a clean fiber cloth includes the following steps: using a NaOH solution to decompose the grease on the surface of the fiber cloth, so that the grease is decomposed into small molecular organic matter; then washing the fiber cloth with acetone to remove the small molecular organic matter on the surface of the fiber cloth; and finally washing other impurities on the fiber cloth with deionized water and / or ethanol.

[0057] In some embodiments, in step 1, a strong oxidant reacts with the fiber cloth under heating conditions at 60-80° C. in a water bath; the strong oxidant is a mixed solution of nitric acid and sulfuric acid or a hydrogen peroxide solution.

[0058] In some embodiments, in step 1, the surface roughened fiber cloth is frozen at a temperature of -60 to -30°C for a freezing time of 10 to 14 hours.

[0059] In some embodiments, in step 4, ammonia water is slowly added dropwise to the reactor and stirred rapidly to ensure that the ammonia water and the ferrous ions on the surface of the fiber cloth can fully and evenly contact and react. If the ammonia water is added too quickly, it may cause the local reaction to be too intense, resulting in a large amount of precipitation, which will affect the uniformity of the reaction. After the ammonia water is added dropwise, the ammonia water and the ferrous ions on the surface of the fiber cloth continue to react for a period of time to ensure that the ammonia water and the ferrous ions fully react.

[0060] In some embodiments, in step five, the pH in the reactor is ≥10, the reaction temperature is 50-80°C, and after the copper ammonia solution or the silver ammonia solution is added dropwise, the reaction is continued at a temperature of 50 to 80°C for a period of time.

[0061] In some embodiments, in step five, hydrogen peroxide, hypochlorite, or persulfate may be added as an oxidant to promote the oxidation of Fe(OH)2.

[0062] Embodiment 1 of the present invention provides a method for preparing a fiber cloth material having a magnetic composite photocatalyst, which comprises the following steps:

[0063] Step 1: Pre-treat the carbon fiber cloth, use 200g 3mol / L sodium hydroxide solution to ultrasonically wash 5g of carbon fiber cloth for 60min, so that the grease on the surface of the carbon fiber cloth is decomposed into small molecular organic matter; then use 100g acetone to ultrasonically wash the carbon fiber cloth for 5min, repeat the washing of the carbon fiber cloth with acetone three times, so as to remove the small molecular organic matter remaining in the carbon fiber cloth. Finally, use 100g deionized water or ethanol aqueous solution (ethanol volume accounts for 50%) to ultrasonically wash the carbon fiber cloth for 5min, repeat three times to remove impurities, and arrange the carbon fiber in a 70℃ blast drying oven for 12h for use.

[0064] Step 2: Roughening and modifying the carbon fiber cloth. Add 100g of strong oxidant aqueous solution to the carbon fiber cloth pretreated in step 1, and stir rapidly in a 75°C water bath to roughen the surface of the carbon fiber cloth. The roughening reaction time is 2 hours. The volume ratio of nitric acid to sulfuric acid in the strong oxidant aqueous solution is 1:3. After the roughening is completed, use deionized water to wash off the strong oxidant, place the fiber arrangement in a -50°C freeze dryer and dry for 12 hours to prepare a carbon fiber cloth with a surface modified with a large number of hydrophilic groups.

[0065] Step 3: Add the carbon fiber cloth to a three-necked flask containing 280g of deionized water, and add 0.25g of sodium dodecylsulfonate and 0.25g of sodium dodecylbenzenesulfonate. Set the water bath heating temperature to 60°C and pass nitrogen to deoxygenate for 30 minutes. Take 2.98g of ferrous chloride tetrahydrate and dissolve it in 20g of deionized water to obtain a ferrous chloride solution. Add the ferrous chloride solution to the three-necked flask, set the stirring speed to 400r / min, and stir for 20min until the ferrous ions and hydrophilic groups are coordinated and balanced. After that, use a peristaltic pump to add 10g of 25% ammonia water dropwise to the three-necked flask, stir rapidly, and the drop time is 10min. After the dropwise addition is completed, react at 60°C for 10min.

[0066] Step 4: Take 0.85g of cupric chloride dihydrate and dissolve it in 10g of deionized water, then add 10g of 25% ammonia water dropwise into the deionized water, a precipitate is generated in the deionized water, and then the precipitate is completely dissolved, and the pH is adjusted to 12 to obtain a copper ammonia solution.

[0067] Step 5: Use a peristaltic pump to add the copper ammonia solution to the three-necked flask and stir rapidly. The addition time is 10 minutes. After the addition is completed, react at 60°C for 30 minutes. During the reaction, the pH must be maintained at 10.

[0068] Step six: After the reaction is completed, the carbon fiber cloth with the magnetic composite photocatalyst is separated by magnetic attraction, and then the carbon fiber cloth is washed with deionized water for 3 times. The carbon fiber with the magnetic composite photocatalyst is placed in a vacuum oven at 60°C and dried for 24 hours. The sample is preserved and named Cu / Fe3O4.

[0069] Embodiment 2 of the present invention provides a method for preparing a fiber cloth material having a magnetic composite photocatalyst, wherein steps 1 to 3 of embodiment 2 are consistent with those of embodiment 1. Embodiment 2 also includes the following steps:

[0070] Step 4: Take 1.7g of silver nitrate and dissolve it in 10g of deionized water, then add 10g of 25% ammonia water dropwise into the deionized water, a precipitate is generated in the deionized water, and then the precipitate is completely dissolved, and the pH is adjusted to 12 to obtain a silver ammonia solution.

[0071] Step 5: Use a peristaltic pump to add the silver ammonia solution to the three-necked flask and stir rapidly. The addition time is 20 minutes. After the addition is completed, react at 60°C for 30 minutes. During the reaction, the pH must be maintained at 10.

[0072] Step six: After the reaction is completed, the carbon fiber cloth with the magnetic composite photocatalyst is separated by magnetic attraction, and then the carbon fiber cloth is washed with deionized water for 3 times. The carbon fiber with the magnetic composite photocatalyst is placed in a vacuum oven at 60°C and dried for 24 hours. The sample is preserved and named Ag / Fe3O4-1.

[0073] Embodiment 3 of the present invention provides a method for preparing a fiber cloth material having a magnetic composite photocatalyst, wherein steps 1 to 3 of embodiment 3 are consistent with those of embodiment 1. Embodiment 3 also includes the following steps:

[0074] Step 4: Take 0.5g of silver nitrate and dissolve it in 10g of deionized water, then add 10g of 25% ammonia water dropwise into the deionized water, a precipitate is generated in the deionized water, and then the precipitate is completely dissolved, and the pH is adjusted to 12 to obtain a silver ammonia solution.

[0075] Step 5: Use a peristaltic pump to add the silver ammonia solution to the three-necked flask, stir rapidly, and add for 20 minutes. After the addition is complete, dissolve 0.54g of potassium persulfate in 5g of deionized water to form a potassium persulfate solution. Then add the potassium sulfate solution to the three-necked flask and react at 60°C for 30 minutes. During the reaction, the pH must be kept at 10.

[0076] Step six: After the reaction is completed, the carbon fiber cloth with the magnetic composite photocatalyst is separated by magnetic attraction, and then the carbon fiber cloth is washed with deionized water for 3 times. The carbon fiber with the magnetic composite photocatalyst is placed in a vacuum oven at 60°C and dried for 24 hours. The sample is preserved and named Ag / Fe3O4-2.

[0077] Comparative Example 1 provides a method for preparing a fiber cloth material with a composite photocatalyst, wherein steps 1 to 2 of Comparative Example 1 are consistent with those of Example 1. Comparative Example 1 also includes the following steps:

[0078] Step 3: Add the carbon fiber cloth to a three-necked flask containing 280g of deionized water, and add 0.25g of sodium dodecylsulfonate and 0.25g of sodium dodecylbenzenesulfonate. Set the water bath heating temperature to 60°C without nitrogen. Take 2.98g of ferrous chloride tetrahydrate and dissolve it in 20g of deionized water to obtain a ferrous chloride solution. Add the ferrous chloride solution to the three-necked flask, set the stirring speed to 400r / min, and stir for 15min until the ferrous ions and the hydrophilic groups are in coordination equilibrium.

[0079] Step 4: Use a peristaltic pump to drop 20g of 25% ammonia water into the three-necked flask, stir rapidly, add for 20 minutes, and slowly introduce air. After the addition is complete, react at 60°C for 60 minutes. During the reaction, the pH must be > 10. Air oxidizes part of Fe(OH)2 to Fe(OH)3, and excess ammonia promotes the reaction of Fe(OH)2 and Fe(OH)3 to Fe3O4.

[0080] Step 5: After the reaction is completed, the carbon fiber cloth with the composite photocatalyst is separated by magnetic attraction, and then the carbon fiber cloth is washed with deionized water for 3 times. The carbon fiber with the photocatalyst is placed in a vacuum oven at 60°C and dried for 24 hours. The sample is preserved and named Fe3O4.

[0081] 1. XRD analysis was performed on the carbon fiber cloth with magnetic composite photocatalyst obtained in Examples 1-3 and the carbon fiber cloth with photocatalyst obtained in Comparative Example 1.

[0082] like Figure 1 As shown, the XRD diffraction peaks of the four samples are at 2θ=35.45°, 43.09°, 56.98°, and 62.58°, corresponding to the (3,1,1), (4,0,0), (5,1,1), and (4,4,0) crystal planes of Fe3O4 in the standard card PDF#03-065-3107, indicating that all four samples have successfully loaded Fe3O4.

[0083] The XRD peak diffraction peaks 2θ=43.41°, 50.56°, and 74.30° of the sample Cu / Fe3O4 in Example 1 correspond to the (1,1,1), (2,0,0), and (2,2,0) crystal planes in the Cu standard card PDF#03-065-9743, respectively, indicating that the sample Cu / Fe3O4 has successfully loaded Cu.

[0084] The XRD peak diffraction peaks 2θ=38.12°, 44.28°, 64.43°, and 77.47° of samples Ag / Fe3O4-1 and Ag / Fe3O4-2 in Examples 2 to 3 correspond to the (1,1,1), (2,0,0), (2,2,0), and (3,1,1) crystal planes in the Ag standard card PDF#04-0783, respectively, indicating that samples Ag / Fe3O4-1 and Ag / Fe3O4-2 have successfully loaded Ag.

[0085] and Figure 1As shown, the four samples have no obvious impurity peaks and are of extremely high purity. The diffraction peaks of Fe3O4 in Examples 1 to 3 are sharper than those in Comparative Example 1, indicating that the Fe3O4 in the samples of Examples 1 to 3 has higher crystallinity. This is because Examples 1 to 3 can quickly oxidize Fe(OH)2 to form Fe(OH)3 through silver / copper ammonium ions, and under water bath heating conditions, Fe(OH)2 and Fe(OH)3 are converted into Fe3O4, resulting in higher crystallinity. Comparative Example 1 uses oxygen as an oxidant, which has a slower oxidation rate and is prone to generate flocculent Fe3O4 with lower crystallinity.

[0086] 2. Carbon fiber cloths with magnetic composite photocatalysts prepared in Examples 1 to 3 and carbon fiber cloth with photocatalysts prepared in Comparative Example 1 were used to photocatalytically degrade Congo red dye and evaluate the photocatalytic performance.

[0087] Take 0.5g of each sample Cu / Fe3O4, sample Ag / Fe3O4-1, sample Ag / Fe3O4-2, and sample Fe3O4 and put them into four beakers containing 100ml of 50mg / L Congo red dye solution, turn on the magnetic stirring device, heat in a 30℃ water bath, and irradiate the beaker with a 300W xenon lamp to simulate visible light. The distance between the beaker and the xenon lamp is 50cm, the photodegradation time is 1h, and the degradation solution is taken every 15min. After adding water to dilute it in a certain proportion, use a UV-visible spectrophotometer to test the absorption value of the solution at 497nm. According to the ratio of the absorbance value of the degradation solution to the absorbance value of the initial solution at different times (i.e., C t / C o )

[0088] like Figure 2 As shown in the figure, all four samples can photocatalytically degrade Congo red dye. This is because under the illumination of the samples, the electrons of the photocatalytic material will jump from the valence band to the conduction band to generate photogenerated electrons and photogenerated holes. When the photogenerated electrons and photogenerated holes encounter water or oxygen, they can generate highly chemically active free radicals such as hydroxyl radicals and superoxide radicals. The active free radicals can destroy the azo bonds in Congo red dye, causing the Congo red dye to degrade.

[0089] The photocatalytic degradation rate and degradation amount of Congo red dye by samples Cu / Fe3O4, sample Ag / Fe3O4-1, and sample Ag / Fe3O4-2 are better than that of sample Fe3O4, indicating that the dispersed distribution of silver / copper in Fe3O4 can significantly improve the photocatalytic performance.

[0090] Cu / Fe3O4 can completely degrade the dye in 15 minutes, and the degradation effect is significantly better than other samples, which proves that Cu / Fe3O4 has an obvious degradation effect on azo dyes under light.

[0091] 3. Carbon fiber cloths with magnetic composite photocatalysts prepared in Examples 1 to 3 and carbon fiber cloth with photocatalysts prepared in Comparative Example 1 were used to photocatalytically degrade Cr(VI) and evaluate the photocatalytic performance.

[0092] Take 0.5g of each sample Cu / Fe3O4, sample Ag / Fe3O4-1, sample Ag / Fe3O4-2, and sample Fe3O4 and put them into four beakers containing 100ml of 20mg / LCr(VI) solution, turn on the magnetic stirring device, heat in a 30℃ water bath, and irradiate the beaker with simulated visible light through a 300W xenon lamp. The distance between the beaker and the xenon lamp is 50cm, the photodegradation time is 1h, and the degradation solution is taken every 15min. After adding water to dilute it in a certain proportion, use a UV-visible spectrophotometer to test the absorption value of the solution at 372nm. According to the ratio of the absorbance value of the degradation solution to the absorbance value of the initial solution at different times (i.e., C t / C o )

[0093] like Figure 3 As shown in the figure, the samples Cu / Fe3O4, Ag / Fe3O4-1 and Ag / Fe3O4-2 can all photocatalytically degrade Cr(VI), while the Fe3O4 sample can hardly photocatalytically degrade Cr(VI). This is because the silver / copper and ferroferric oxide form a Schottky junction structure, that is, a built-in potential difference is formed on the contact surface between the silver / copper and ferroferric oxide. The built-in potential difference can transfer the electrons on the ferroferric oxide to the silver / copper, thereby effectively separating the electron-hole pairs and further improving the photocatalytic ability of the composite material.

[0094] The photocatalytic degradation effect of sample Cu / Fe3O4 on Cr(VI) is better than that of samples Ag / Fe3O4-1 and Ag / Fe3O4-2. This is because the built-in potential difference between Fe3O4 and Cu is significantly higher than the built-in potential difference between Fe3O4 and Ag, which can more significantly and effectively separate electron-hole pairs.

[0095] The photocatalytic degradation effect of sample Ag / Fe3O4-2 on Cr(VI) is better than that of sample Ag / Fe3O4-1, indicating that the magnetic composite photocatalyst contains a larger proportion of Ag and a smaller proportion of Fe3O4, which will weaken the photocatalytic degradation effect on Cr(VI).

[0096] 4. The carbon fiber cloth with magnetic composite photocatalyst prepared in Examples 1 to 3 and the carbon fiber cloth with photocatalyst prepared in Comparative Example 1 were evaluated for photocatalytic antibacterial performance.

[0097] The concentration of bacterial solution was 1×10 7100 μL of E. coli solution with cfu / mL was evenly spread on a sterile nutrient agar plate. 5mm·5mm carbon fiber cloth of four samples was attached to the agar plate, and 20 μL of sterile saline was added to each carbon fiber cloth to increase the adhesion between the fiber cloth and the agar plate. After the plate was sealed, it was placed under natural light at 37℃ for 12 hours, and the size of the inhibition zone of the four samples was observed.

[0098] like Figure 5 As shown, position 1 is sample Cu / Fe3O4, position 2 is sample Ag / Fe3O4-1, position 3 is sample Ag / Fe3O4-2, position 4 is sample Fe3O4, and position 5 is carbon fiber cloth. Escherichia coli can contaminate carbon fiber cloth without photocatalyst. Compared with the carbon fiber cloth at position 5, sample Cu / Fe3O4 produces a larger inhibition zone, sample Ag / Fe3O4-2 produces a smaller inhibition zone, and the inhibition zones produced by samples Ag / Fe3O4-1 and Fe3O4 are not obvious, indicating that the four samples can produce antibacterial effects through photocatalysis, among which sample Cu / Fe3O4 has the best antibacterial performance, followed by sample Ag / Fe3O4-2, which is highly similar to the effect of carbon fiber cloth with magnetic composite photocatalysis on degrading heavy metals, indicating that the antibacterial effect is mainly affected by photogenerated electrons and holes, and is less affected by the content of Cu and Ag.

[0099] Therefore, the magnetic composite photocatalytic fiber cloth of the present invention is applied to the field of fabrics for daily use, which can significantly improve the antibacterial property and self-cleaning property of the fabrics and extend the service life of the fabrics, and has potential application value.

[0100] 5. The carbon fiber cloth with magnetic composite photocatalyst obtained in Examples 1 to 3 and the carbon fiber cloth with photocatalyst obtained in Comparative Example 1 were subjected to electrochemical impedance spectroscopy test. The results are as follows Figure 4 As shown in the figure, the radius of the Nyquist curve arc decreases in the order of Fe3O4, Ag / Fe3O4-1, Ag / Fe3O4-2, and Cu / Fe3O4, which means that the smaller the electrochemical impedance of the sample Fe3O4, the sample Ag / Fe3O4-1, the sample Ag / Fe3O4-2, and the sample Cu / Fe3O4, the higher the migration rate of the photogenerated electrons and holes in the sample in this order. This is because the driving force generated by the Schottky junction between the Fe3O4 and Ag / interface can effectively reduce the impedance inside the material, accelerate the directional migration rate of the photogenerated electrons and holes, and inhibit the recombination of the photogenerated electron-hole pairs. The electrochemical impedance analysis results are highly consistent with the photocatalytic results, proving that the dispersed composite photocatalyst structure effectively improves the photocatalytic efficiency.

[0101] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A fiber cloth material with a magnetic composite photocatalyst, characterized in that: The invention comprises a fiber cloth with a roughened surface, wherein the surface of the fiber cloth with a roughened surface is loaded with a magnetic composite photocatalyst, wherein the magnetic composite photocatalyst comprises ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

2. The method for preparing a fiber cloth material having a magnetic composite photocatalyst according to claim 1, characterized in that: The mass fraction of ferrosoferric oxide in the magnetic composite photocatalyst is greater than the mass fraction of copper and / or silver.

3. The method for preparing a fiber cloth material having a magnetic composite photocatalyst according to claim 1, characterized in that: The copper and / or silver are dispersed in the ferroferric oxide to form nano-scale magnetic composite photocatalytic particles.

4. A method for preparing a fiber cloth material having a magnetic composite photocatalyst, for preparing the fiber cloth material having a magnetic composite photocatalyst according to any one of claims 1 to 3, characterized in that: A fiber cloth with a roughened surface and modified with hydrophilic groups is used, and the surface of the fiber cloth is modified with ferrous ions through the coordination effect between the hydrophilic groups and ferrous ions; the ferrous ions on the surface of the fiber cloth are then converted into Fe(OH)2; and then a magnetic composite photocatalyst is generated on the surface of the fiber cloth through the reaction of Fe(OH)2 with a copper ammonia solution or Fe(OH)2 with a silver ammonia solution. The magnetic composite photocatalyst includes ferroferric oxide, copper and / or silver, and the copper and / or silver are dispersed in the ferroferric oxide.

5. The method for preparing a fiber cloth material having a magnetic composite photocatalyst according to claim 4, comprising the following steps: Step 1: placing a clean fiber cloth into an aqueous solution containing a strong oxidant to roughen the surface of the fiber cloth; then freeze-drying the fiber cloth with the roughened surface to obtain a fiber cloth with hydrophilic groups on the surface; Step 2: Add deionized water and anionic surfactant into the reactor, then add fiber cloth containing hydrophilic groups, heat in a water bath and stir rapidly; Step 3: Adding a ferrous salt aqueous solution into the reactor, the ferrous ions coordinate with the hydrophilic groups of the fiber cloth, so that the ferrous ions on the surface of the fiber cloth; Step 4: Slowly add ammonia water into the reactor, and the ferrous ions on the surface of the fiber cloth will generate flocculent Fe(OH)2 in an alkaline environment; Step 5: slowly dripping a copper ammonia solution or a silver ammonia solution into the reactor as an oxidant to react with the flocculent Fe(OH)2 on the surface of the fiber cloth to generate a fiber cloth material with a magnetic composite photocatalyst; Step 6: Magnetic absorption collects the fiber cloth material with magnetic composite photocatalyst in step 5, and washes and dries it; In step 3, step 4 and step 5, the reactor is in an oxygen-free state.

6. The method for preparing a magnetic composite fiber cloth visible light catalytic material according to claim 5, characterized in that: In step 1, the preparation of clean fiber cloth includes the following steps: using NaOH solution to decompose the grease on the surface of the fiber cloth, so that the grease is decomposed into small molecular organic matter; then washing the fiber cloth with acetone to wash away the small molecular organic matter on the surface of the fiber cloth; finally, washing the fiber cloth with deionized water and / or ethanol to remove other impurities.

7. The method for preparing a magnetic composite fiber cloth visible light catalytic material according to claim 5, characterized in that: In the step 1, a strong oxidant reacts with the fiber cloth under heating conditions at 60-80° C. in a water bath; the strong oxidant is a mixed solution of nitric acid and sulfuric acid or a hydrogen peroxide solution.

8. The method for preparing a magnetic composite fiber cloth visible light catalytic material according to claim 5, characterized in that: In the step 1, the freezing temperature of the roughened fiber cloth is -60 to -30°C, and the freezing time is 10 to 14 hours.

9. The method for preparing a magnetic composite fiber cloth visible light catalytic material according to claim 5, characterized in that: In the step 4, ammonia water is slowly added to the reactor and stirred rapidly. After the addition of ammonia water is completed, the ammonia water continues to react with the ferrous ions on the surface of the fiber cloth for a period of time.

10. The method for preparing a magnetic composite fiber cloth visible light catalytic material according to claim 9, characterized in that: In the step 5, the pH in the reactor is ≥ 10, the reaction temperature is 50-80° C., and after the copper ammonia solution or the silver ammonia solution is added dropwise, the reaction is continued for a period of time; Alternatively, after the copper ammonia solution or silver ammonia solution is added dropwise, hydrogen peroxide, hypochlorite or persulfate is added as an oxidant, and the reaction is continued at the temperature for a period of time.