Flexible pH sensor based on conductive polymer layer and preparation method thereof
By introducing Ti4O7 and sulfate-containing ions into the conductive polymer layer pH sensor and using activated three-dimensional flexible carbon materials, the problem of insufficient stability and sensitivity of the sensor in the physiological environment is solved, and high sensitivity and long-term stability in physiological media are achieved pH detection.
Patent Information
- Application Number
- CN202411151686.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The application of existing conductive polymer layer pH sensors in the field of biomedical medicine is limited by their paranormal response, low sensitivity, limited chemical stability and insufficient mechanical strength, resulting in poor stability in service in physiological environments for a long time, making it difficult to achieve early stage. Detection and continuous monitoring.
Using a three-dimensional flexible substrate including Ti4O7, sulfate ions and conductive polymer materials, a conductive polymer layer is prepared by electrochemical deposition to form a stable conductive polymer layer, which enhances the chemical stability and sensitivity of the sensor, and activates the three-dimensional Flexible carbon materials improve the mechanical strength and sensitivity of the sensor.
The pH detection with high sensitivity and long-term stability in physiological media is achieved, and the sensor maintains good responsiveness within 90 days, suitable for continuous monitoring of wearable and implantable environments.
Smart Images

Figure CN118961840A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biosensors, and in particular relates to a flexible pH sensor based on a conductive polymer layer and a preparation method thereof. Background Art
[0002] pH is crucial for many chemical and biological reactions. Some physiological processes, such as implant degradation, microbial infection, tumor metastasis, and wound healing, can determine the status of these processes through changes in pH. Once deviations occur, pH will reliably show abnormalities and diseases. At present, many materials have been developed for pH sensing, such as glass electrodes, modern extended gate field effect transistor (EGFET) pH sensors, ion field effect transistor (ISFET) pH sensors, optical fiber pH sensors, hydrogel membranes, etc. However, these technologies still have disadvantages in the field of healthcare, such as rigidity, high cost, short battery life, and cytotoxicity.
[0003] Patent CN117554447A discloses a method for preparing a flexible conductive polymer layer pH sensor, the specific steps are: first, prepare a printed anode flexible film, and then realize the synthesis of a metal-doped polyaniline composite material on its surface by cyclic voltammetry. This method can achieve high bending stability, but there is no test to reflect its long-term service stability. Patent CN117990657A discloses an optical fiber pH value detection method using a polyaniline reaction deposition film layer, which uses the change in refractive index of the polyaniline sensitive film after contact with the liquid to be tested. The swept frequency laser is reflected by the optical fiber pH sensor and then incident on the fiber grating demodulator for spectral extraction, and the pH value of the liquid to be tested is obtained by analysis and processing. The preparation method of this invention is complex and costly, and it cannot achieve long-term continuous monitoring in a wearable / implantable environment. Patent CN113670999A discloses a metal oxide-based pH sensing electrode and its preparation method and application, which is electrochemically directed to WO 3- H intercalated in the lattice + , and transform its crystal structure from monoclinic phase to cubic phase, which greatly improves its conductivity, thereby improving the ion-electron conversion efficiency of the sensing layer. However, this method requires the addition of adhesives and is also difficult to meet the requirements of long-term continuous monitoring in wearable / implantable environments.
[0004] Although many types of pH sensors have been developed, there is still a lack of practical applications in the biomedical field. Conductive polymer materials show very good pH sensing potential due to their excellent electrochemical properties. Their high biocompatibility, flexibility, stretchability, antibacterial properties, antioxidant properties, and easy deposition on any flexible substrate give them unique biomedical application potential. So far, conductive polymer layer pH sensors have mainly developed in the direction of nano-sizing and multi-component composites. However, the main bottlenecks that hinder the widespread application of conductive polymer materials in the field of biomedical sensing are as follows: on the one hand, many conductive polymer layer pH sensors only have sub-Nernstian response and low sensitivity. Especially when used for designated small range detection, pH sensitivity is particularly important, such as accuracy at neutral pH, which is particularly meaningful for physiological measurements. On the other hand, for practical applications, these polymers have limited chemical stability and low mechanical strength. The sensitivity of the sensor is difficult to maintain stability for a long time in situ or in vivo, the service life is short, and the potential drift is serious, so that its advantages cannot be well utilized. Therefore, it is of great practical significance to improve its chemical stability and develop pH sensors with long-term stability for early detection of pH fluctuations and abnormal conditions when implanted in or on the surface of organisms. Summary of the invention
[0005] The purpose of the present invention is to provide a flexible pH sensor based on a conductive polymer layer and a preparation method thereof, so as to improve the long-term stability of the pH sensor and solve the technical problems that conductive polymer materials are easy to degrade and have a short service life when used for pH sensing.
[0006] To achieve the above objectives, the present invention provides a flexible pH sensor based on a conductive polymer layer, comprising a three-dimensional flexible substrate and a conductive polymer layer deposited on the surface of the three-dimensional flexible substrate; the conductive polymer layer comprises Ti4O7, sulfur-containing acid ions and a conductive polymer material.
[0007] Furthermore, the Ti4O7 is hydroxylated Ti4O7, and there is a chemical bonding reaction between the hydroxylated Ti4O7 and the sulfur-containing acid radical ion;
[0008] The sulfur-containing acid radical ions are derived from sulfuric acid, sulfonic acid, or sulfonate, for example, one or more of sulfuric acid, sodium p-toluenesulfonate, sodium polystyrenesulfonate, sodium dodecylbenzenesulfonate, and β-naphthalenesulfonic acid, preferably sodium p-toluenesulfonate.
[0009] Further, the three-dimensional flexible substrate is a three-dimensional flexible conductive substrate, preferably a three-dimensional flexible carbon substrate; the three-dimensional flexible carbon substrate includes carbon nanotubes, graphene, carbon paper, natural carbon fiber, carbon cloth, foam carbon or MXene, preferably foam carbon;
[0010] The conductive polymer material includes one or more of polypyrrole, polyaniline and polythiophene, preferably polypyrrole.
[0011] The present invention also provides a method for preparing a flexible pH sensor based on a conductive polymer layer as described in any of the above items, comprising: preparing a deposition liquid containing Ti4O7, sulfur-containing acid ions and conductive polymer material monomers, and depositing them on a three-dimensional flexible substrate to obtain a flexible pH sensor.
[0012] Furthermore, the preparation method of the deposition liquid includes: hydroxylating Ti4O7, then reacting with sulfur-containing acid radical ions to obtain sulfur-containing acid radical ion-modified Ti4O7, and then adding the monomer corresponding to the conductive polymer material to obtain the deposition liquid.
[0013] Furthermore, the preparation method of the deposition liquid is as follows: the hydroxylation adopts methanesulfonic acid; the average particle size of the Ti4O7 is 100 to 500 nm.
[0014] Furthermore, the deposition liquid is deposited on the three-dimensional flexible substrate by electrochemical deposition; the electrochemical deposition method uses the three-dimensional flexible substrate as a working electrode, a saturated calomel electrode as a reference electrode, a platinum sheet as a counter electrode, and the deposition liquid as an electrolyte solution.
[0015] Furthermore, the concentration of the conductive polymer monomer in the deposition solution is 0.1-1 mol / L, the concentration of Ti4O7 is 10-50 g / L, and the concentration of the sulfur-containing acid radical ion is 0.1-5 mol / L. The conductive polymer monomer includes pyrrole, aniline or thiophene.
[0016] Furthermore, the electrochemical deposition method adopts constant current, constant potential or pulse electrodeposition, preferably constant current; the power consumed per square centimeter of electrode surface is 8 to 12C.
[0017] Furthermore, the three-dimensional flexible carbon substrate is a substrate activated by an activator, and the activator is one of sulfuric acid, nitric acid, phosphoric acid, potassium hydroxide, potassium carbonate, and zinc chloride; preferably 4 to 8 mol / L sulfuric acid. The temperature of the activation treatment is 80 to 160°C, and the time is 4 to 8 hours. The three-dimensional flexible carbon substrate can also be activated by a physical activation method, such as plasma etching.
[0018] The method for preparing a flexible pH sensor based on a conductive polymer layer of the present invention specifically comprises:
[0019] (1) A three-dimensional flexible porous carbon substrate with rich oxygen-containing functional groups on its surface is obtained by activation modification;
[0020] (2) preparing dopant particles Ti4O7 powder by Ti reduction method;
[0021] (3) A ternary composite pH sensing electrode consisting of Ti4O7, conductive polymer layer and three-dimensional flexible porous carbon substrate was prepared in one step by an electrochemical method.
[0022] In some embodiments, step (1) uses a chemical activation method to prepare modified three-dimensional flexible carbon, including: first, using deionized water, ethanol, and acetone to ultrasonically clean the three-dimensional flexible carbon substrate, and drying it for use. Take 2 to 3 clean three-dimensional flexible carbon electrodes and add them to 10mL of chemical activator prepared in a certain proportion. After mixing and impregnating for a period of time, transfer them to a 50mL polytetrafluoroethylene reactor liner, place them at a certain temperature for a certain period of time for hydrothermal reaction, and after cooling to room temperature, take out the samples, rinse them with ethanol and acetone, and dry them for use, so as to obtain modified three-dimensional flexible carbon.
[0023] Step (2) uses a Ti reduction method to prepare Ti4O7 powder, including: weighing a certain mass ratio of Ti and TiO2 (the mass ratio of TiO2 to Ti is 7:(1-2)), grinding them evenly in an agate mortar, and then putting the mixed powder into a tube furnace, heating it to a certain temperature at a certain heating rate under an Ar environment, and calcining it for a certain time (4-8h). After the calcination is completed, wait for the furnace temperature to cool naturally to room temperature, take out the sample powder that has turned into black, that is, the product Ti4O7, and package it for later use after grinding.
[0024] In some embodiments, step (2) hydroxylates the prepared Ti4O7 powder, and uniformly disperses the modified Ti4O7 particles and the sulfur-containing acid radical ion solution, specifically comprising:
[0025] The Ti4O7 particles obtained by the above steps are etched and activated with methanesulfonic acid to make their surface rich in hydroxyl groups, which serve as active sites for subsequent reactions. That is, a certain amount of Ti4O7 particles is added to 100mL of methanesulfonic acid diluted to a certain concentration, and stirred and refluxed for 24 hours. The modified Ti4O7 particles are centrifuged, washed with distilled water, and dried in an oven at 60°C for 24 hours. Then a certain mass of modified Ti4O7 particles is added to a sulfur-containing acid radical ion solution and stirred. In this process, the hydroxyl groups on the surface of the Ti4O7 particles fully react with the sulfur-containing groups in the solution.
[0026] Preferably, the concentration of Ti4O7 in the synthetic solution is 10-50 g / L, and the concentration of the sulfur-containing acid radical ion p-toluenesulfonic acid is 0.1-5 mol / L.
[0027] In some embodiments, step (3) uses an electrochemical method to uniformly deposit the composite on the modified three-dimensional flexible carbon substrate to obtain a ternary composite pH sensor, which specifically includes:
[0028] Take 100 mL of the sulfur-containing acid radical ion-modified Ti4O7 mixed solution of step (2), add the corresponding monomer of the conductive polymer and pass N2 for 10 minutes to degas the polymer solution as the electrolyte solution. The synthesis uses a traditional three-electrode system, the modified three-dimensional flexible carbon prepared in step (1) is used as the working electrode, the counter electrode uses a platinum sheet (2×2 cm), and the reference electrode is a saturated calomel electrode (SCE) with a glass salt bridge. The electrochemical deposition process is achieved using a Gmary 3000 electrochemical workstation. The entire deposition process is carried out under low-speed stirring. After the deposition is completed, the obtained ternary complex is washed with deionized water and dried naturally for use.
[0029] According to another aspect of the present invention, there is also provided a pH sensor with long-term stability for use in early detection of pH fluctuations and abnormal conditions in implants or on the surface of biological bodies, thereby achieving accurate measurement of pH values in common physiological media and stability of long-term continuous operation in situ or in vivo.
[0030] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:
[0031] 1. According to the calculation of density functional theory (DFT), the new ceramic material Ti4O7 can produce a strong bonding effect with various sulfur elements. Therefore, the present invention bonds the new ceramic material Ti4O7 with sulfur-containing acid ions, and the sulfur-containing acid ions are then combined with the conductive polymer material through electrostatic action, thereby stabilizing the doped ions in the conductive polymer layer, inhibiting the collapse of the conductive polymer layer, effectively delaying the degradation of the conductive polymer layer, and improving the long-term stability.
[0032] 2. The conductive polymer layer proposed by the present invention includes Ti4O7, sulfur-containing acid ions and conductive polymer materials. The conductive polymer materials can undergo reversible protonation-deprotonation reactions. At the same time, the conjugated structure allows the π electrons to move freely in the energy band shared by the entire molecule, making it have good conductivity, so that it can be used for high sensitivity and rapid detection of the pH value of the solution. At the same time, the conductive polymer layer has good antibacterial and antioxidant properties, which is conducive to the application in implantable / wearable medical care.
[0033] 3. After activation and modification, the three-dimensional flexible carbon material has abundant oxygen-containing functional groups on its surface, which can form hydrogen bonds with N, O, etc. in the conductive polymer layer, which is beneficial to the directional arrangement of the conductive polymer chain, thereby improving the electronic transmission efficiency and structural stability of the polymer, and further promoting the improvement of conductivity and. At the same time, due to the large specific surface area and high porosity of the three-dimensional flexible carbon material, it has abundant active sites, which can greatly increase the sensing area and sensing sensitivity. In addition, the three-dimensional flexible carbon material also gives the conductive polymer layer pH sensor the advantages of good flexibility and customizable electrode shape and area.
[0034] 4. The pH sensor based on the conductive polymer layer prepared by the present invention improves the stability of the conductive polymer layer by modifying the new ceramic material Ti4O7, so that the pH sensor not only has excellent pH sensing ability and can achieve super-Nernstian response, but also can maintain good response ability after long-term service for 90 days.
[0035] 5. The electrochemical method used in the present invention has a simple preparation and synthesis process, a stable process, and the raw materials used can be directly purchased on the market and are easily available, thus having broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 In the figure, a, b, c, and d are scanning electron microscope images of the new ceramic material Ti4O7, the activated foam carbon substrate prepared in Examples 1 and 2, the ternary composite electrode in Example 1, and the binary composite electrode in Example 2, respectively.
[0037] Figure 2 This is a graph showing the results of pH responsiveness changes during 90 days of service in 37°C human body simulation fluid in Examples 1-2.
[0038] Figure 3 This is a graph showing the result of the open circuit potential fluctuation during the 90-day service period in 37° C. human body simulation fluid in Examples 1-2.
[0039] Figure 4 These are scanning electron microscope images of Example 1 at different scales after being immersed in 37°C human body simulation fluid for 90 days.
[0040] Figure 5 These are scanning electron microscope images of Example 2 at different scales after being immersed in 37°C human body simulation fluid for 90 days. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0042] The flexible pH sensor based on a conductive polymer layer provided by the present invention is used as a main sensing unit in practical applications. The pH sensor is a ternary composite electrode composed of a modified three-dimensional flexible substrate loaded with a new ceramic material Ti4O7 and a conductive polymer layer.
[0043] The present invention preferably uses modified three-dimensional porous flexible carbon materials as conductive supports to support active materials, improves the sensing area, conductivity and stability of the sensing materials, and realizes the flexibility and customizable design appearance requirements of the composite electrode; a new ceramic material Ti4O7 (one of the Magn'eli phases, Ti) with excellent conductivity and dielectric chemical inertness is used. n O 2n-1 , n≥4) as a composite material to enhance the dielectric stability of the conductive polymer layer, thereby greatly improving the long-term stability of the composite pH sensor and solving the technical problems of easy degradation and short service life of conductive polymer materials used for pH sensing.
[0044] The method for preparing a pH sensor based on a conductive polymer layer of the present invention comprises the following steps:
[0045] (1) Preparation of modified three-dimensional flexible carbon materials by chemical activation method;
[0046] (2) preparing Ti4O7 powder by Ti reduction method, then hydroxylating it, and mixing and dispersing the hydroxylated Ti4O7 particles with sulfur-containing acid radical ion solution to perform chemical bonding;
[0047] (3) A conductive polymer layer doped with Ti4O7 particles is grown on the modified three-dimensional flexible carbon material prepared in step (1) by an electrochemical method, thereby obtaining a ternary composite pH sensor.
[0048] The electrochemical method uses the modified three-dimensional porous flexible carbon material as the working electrode, the saturated calomel electrode as the reference electrode, the platinum sheet as the counter electrode, and the monomer corresponding to the conductive polymer, the sulfur-containing acid radical ions, and the mixed solution of the new ceramic material Ti4O7 as the electrolyte solution. The concentration of the monomer corresponding to the conductive polymer material in the electrolyte solution is 0.1-1 mol / L, the concentration of the Ti4O7 is 10-50 g / L, and the concentration of the sulfur-containing acid radical ions is 0.1-1 mol / L.
[0049] When the ternary complex sensing electrode is in a medium with different pH values, it shows different open circuit potential values, and the change of the medium pH value can be monitored according to the different potential values. The present invention can monitor the change of the medium pH value according to the different potential values within a use period of up to 90 days, meeting the accuracy of small-scale pH measurement in physiological media and the stability during long-term continuous operation in situ or in vivo. At the same time, the pH sensor has the advantages of good flexibility, customizable electrode shape and area, and no cytotoxicity.
[0050] It should be noted that, since the conductive polymer material itself has conductivity and pH responsiveness, the three-dimensional flexible substrate of the present invention is not limited to the three-dimensional flexible carbon material, that is, by preparing a deposition solution containing Ti4O7, sulfur-containing acid ions and monomers corresponding to the conductive polymer material, depositing on the three-dimensional flexible substrate to obtain a flexible pH sensor, the effect of long-term stability can also be achieved. When the activated three-dimensional flexible carbon material is preferred, it is conducive to the directional arrangement of the conductive polymer chain, thereby improving the electronic transmission efficiency and structural stability of the conductive polymer, and further promoting the improvement of conductivity and stability.
[0051] Example 1
[0052] A pH sensor based on a conductive polymer with long-term stability is prepared by the following method:
[0053] Step 1: Prepare modified activated carbon foam by chemical activation
[0054] First, use deionized water, ethanol, and acetone to ultrasonically clean the foam carbon substrate (1×1 cm), and dry it for use. Prepare 8 mol / L H2SO4 aqueous solution, take 2 to 3 cleaned foam carbon electrodes and add them to the prepared 10 mL H2SO4 solution, put them into a 50 mL polytetrafluoroethylene reactor for hydrothermal reaction, the hydrothermal temperature is 120 ° C, the hydrothermal time is 4 hours, and after cooling to room temperature, take out the sample, rinse it with ethanol and acetone, and dry it to obtain the activated foam carbon electrode for use.
[0055] Step 2: Prepare Ti4O7 powder by Ti reduction method
[0056] Weigh TiO2 and Ti powder in a mass ratio of 7:1, grind them evenly in an agate mortar, then put the mixed powder into a tubular furnace, heat it to 850℃ at a certain heating rate in an Ar environment and calcine it for 4 hours. After the calcination is completed, wait for the furnace temperature to cool naturally to room temperature, take out the sample powder that has turned into black, that is, the product Ti4O7, and package it after grinding for later use. Then add the Ti4O7 particles to 100mL of diluted methanesulfonic acid and stir and reflux for 24 hours. After centrifugation, the modified Ti4O7 particles are washed with distilled water and dried in an oven at 60℃ for 24 hours. Then 5g of modified Ti4O7 particles are added to 100mL of 0.1M sodium p-toluenesulfonate (pTS) solution (the solvent is water) and stirred. In this process, the hydroxyl groups on the surface of the Ti4O7 particles react with the pTS in the solution. - The reaction is sufficient to form a pTS-Ti4O7 composite solution with strong interaction force.
[0057] Step 3: Distill and purify the pyrrole monomer
[0058] Take 100 mL of pyrrole monomer in a 150 mL round-bottom flask, add 2 to 3 zeolites, distill and purify, collect the purified pyrrole solution and store it in a refrigerator in the dark.
[0059] Step 4: The composite is uniformly deposited on the activated carbon foam substrate by electrochemical method. The obtained ternary composite is recorded as Ti4O7+PPy / ACF
[0060] Take 100 mL of the pTS-Ti4O7 composite solution from step 2, add pyrrole monomer to it to a concentration of 0.1 M, and pass N2 for 10 min to degas the polymer solution to obtain an electrolyte solution. The synthesis uses a traditional three-electrode system, with the activated carbon foam prepared in step 1 as the working electrode, a platinum sheet (2×2 cm) as the counter electrode, and a saturated calomel electrode (SCE) with a glass salt bridge as the reference electrode. The electrochemical deposition process was carried out using a constant current deposition method in a Gmary 3000 electrochemical workstation, with a deposition current density of 4 mA cm -2 The deposition time was 2000s. The entire deposition process was carried out under low-speed stirring. After the deposition, the obtained ternary composite was washed with deionized water and dried naturally for use. The scanning electron microscope image of the prepared ternary composite electrode Ti4O7+PPy / ACF is shown in Figure 1 As shown in c.
[0061] Example 2
[0062] The difference between this embodiment and embodiment 1 is that after the three-dimensional flexible foam carbon substrate is chemically activated, only sulfuric acid is doped when the conductive polymer layer is grown by electrochemical method, and the new ceramic material Ti4O7 is not doped (that is, the electrolyte solution is composed of only 0.1M conductive polymer pyrrole monomer and 0.1M sodium p-toluenesulfonate). The obtained product is recorded as a binary composite electrode PPy / ACF, and its scanning electron microscope image is as follows Figure 1 As shown in middle d.
[0063] Test Example 1
[0064] Long-term service behavior of simulated samples in human body simulated fluid at 37℃
[0065] The samples prepared in Examples 1 and 2 were fixed with working electrode clamps and the sides were sealed with silicone rubber, leaving only 1 cm 2 The working surface is then immersed in 150 mL of human body simulation fluid at 37°C, and 150 mL of fresh simulation fluid is replaced every 7 days to simulate the dynamic body fluid of the human body. The human body simulation fluid is mainly composed of sodium chloride, potassium chloride, magnesium chloride, calcium chloride, sodium bicarbonate, potassium dihydrogen phosphate, and magnesium sulfate. The prepared solution is adjusted to pH 7.2-7.4 with 0.1M sodium hydroxide and stored at room temperature for use.
[0066] (1) pH responsiveness changes of Examples 1 to 2 in human body simulated fluid:
[0067] The changes in pH responsiveness of Examples 1 to 2 in human body simulated fluid are as follows: Figure 2 As shown, Figures a and c refer to the open circuit potential and its linear fitting of Examples 1 and 2 taken out and tested in solutions with different pH values after being immersed for 0, 7, 30, 60 and 90 days, respectively, and Figures b and d refer to the slope fluctuation of the electrode potential of Examples 1 and 2 as the pH value changes after being immersed for 0, 7, 30, 60 and 90 days, respectively.
[0068] When polypyrrole undergoes a reversible protonation-deprotonation reaction of nitrogen atoms in a solution, it can be described by the following equation:
[0069]
[0070] The degradation of polypyrrole causes the structure to transform into a quinone structure, accompanied by the removal of doped ions. When the degradation time is long enough, the quinone structure will be further hydrolyzed and undergo a ring-opening reaction to generate the final degradation products, including C=O, C=N and -CH=CH-. Its electrochemical activity and conductivity will be irreversibly degraded, resulting in the loss of pH responsiveness. Figure 2 It can be seen that both newly prepared composite electrodes have good performance, but the PPy / ACF electrode loses some sensitivity, has poor linear fit, and has large individual differences during the 90-day immersion period (the error bar in Figure d is larger). The Ti4O7+PPy / ACF electrode can maintain the Nernst response during the 90-day service period.
[0071] (2) Other response performance changes of Examples 1 to 2 in human body simulation fluid:
[0072] Other responsiveness tests of the two newly prepared composite electrodes in human body simulation fluid, including electrode response time test, repeatability test, reversibility test, interfering ion selectivity test, stability test, etc., all show that the two composite electrodes have excellent performance in these aspects. After 90 days of service, the same responsiveness test was performed again. Except for a slightly prolonged response time, the Ti4O7+PPy / ACF electrode had no significant difference from before immersion in other aspects, indicating that it can maintain good performance during the 90-day service period. After immersion, the response time of the PPy / ACF electrode became significantly longer, and the potential deviation and potential drift were serious.
[0073] (3) Open circuit potential fluctuations of Examples 1 and 2 in human body simulated fluid:
[0074] The open circuit potential changes of the composite electrode in human body simulated fluid are as follows: Figure 3As shown, the potential change rules of the two sensors are basically the same, and there is an activation period in which the potential continues to rise within the first seven days. Then, in the following long period of time, the electrode experiences a small potential fluctuation. The fluctuation of the PPy / ACF electrode is within 20mV within 60 days, while the Ti4O7+PPy / ACF electrode fluctuates within 17mV within a longer period of 80 days, and the error bar of Ti4O7+PPy / ACF reflects that the individual differences between the electrodes in the group are smaller. It shows that the conductive polymer layer ternary composite pH sensor of the present invention has basically no sensitivity loss within 90 days, and the performance test meets the requirements.
[0075] Test Example 2
[0076] The morphology of Examples 1 and 2 after being immersed in 37°C human body simulation fluid for different time periods
[0077] The surface morphology of the composite electrode after immersion in human body simulation fluid for 90 days was photographed by scanning electron microscope. Figure 4 and 5 As shown in the figure, compared with the PPy / ACF electrode, the PPy still maintains its original morphology, and a large amount of Ti4O7 powder remains on the surface, and the electrode integrity is good.
[0078] In summary, the pH sensor based on the conductive polymer layer prepared by the present invention not only has excellent pH sensing ability, can achieve super-Nernst response, and has anti-ion interference ability, but also has excellent response time, electrode repeatability, reversibility and stability. After 90 days of long-term service, the electrode still has good response ability, and the response slope is maintained at 59mV / pH and above. Therefore, the pH sensor of the present invention can monitor the change of pH value according to different potential values during the use time of up to 90 days, and realize the accurate measurement of pH value in common physiological media and the stability of long-term continuous operation in situ or in vivo.
[0079] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A flexible pH sensor based on a conductive polymer layer, characterized in that: It comprises a three-dimensional flexible substrate and a conductive polymer layer deposited on the surface of the three-dimensional flexible substrate; the conductive polymer layer comprises Ti4O7, sulfur-containing acid radical ions and conductive polymer materials.
2. The flexible pH sensor based on a conductive polymer layer according to claim 1, characterized in that: The Ti4O7 is hydroxylated Ti4O7, and there is a chemical bonding reaction between the hydroxylated Ti4O7 and the sulfur-containing acid radical ion; The sulfur-containing acid radical ions are derived from one or more of sulfuric acid, sodium p-toluenesulfonate, sodium polystyrenesulfonate, sodium dodecylbenzenesulfonate, and β-naphthalenesulfonic acid, preferably sodium p-toluenesulfonate.
3. The flexible pH sensor based on a conductive polymer layer according to claim 1, characterized in that: The three-dimensional flexible substrate is a three-dimensional flexible conductive substrate, preferably a three-dimensional flexible carbon substrate; the three-dimensional flexible carbon substrate is carbon nanotubes, graphene, carbon paper, natural carbon fiber, carbon cloth, foam carbon or MXene material, preferably foam carbon; The conductive polymer material is one or more of polypyrrole, polyaniline and polythiophene, preferably polypyrrole.
4. A method for preparing a flexible pH sensor based on a conductive polymer layer according to any one of claims 1 to 3, characterized in that: include: A deposition solution containing Ti4O7, sulfur-containing acid radical ions and monomers corresponding to the conductive polymer material is prepared and deposited on a three-dimensional flexible substrate to obtain a flexible pH sensor.
5. The preparation method according to claim 4, characterized in that: The preparation method of the deposition liquid comprises: hydroxylating Ti4O7, then reacting with sulfur-containing acid radical ions to obtain Ti4O7 modified with sulfur-containing acid radical ions, and then adding monomers corresponding to the conductive polymer material to obtain the deposition liquid.
6. The preparation method according to claim 5, characterized in that: The hydroxylation adopts methanesulfonic acid; the average particle size of the Ti4O7 is 100-500nm.
7. The preparation method according to claim 6, characterized in that: In the deposition solution, the concentration of the monomer corresponding to the conductive polymer material is 0.1-1 mol / L, the concentration of the Ti4O7 is 10-50 g / L, and the concentration of the sulfur-containing acid radical ions is 0.1-5 mol / L.
8. The preparation method according to any one of claims 4 to 7, characterized in that: The deposition liquid is deposited on the three-dimensional flexible substrate by electrochemical deposition; the electrochemical deposition method uses the three-dimensional flexible substrate as a working electrode, a saturated calomel electrode as a reference electrode, a platinum sheet as a counter electrode, and the deposition liquid as an electrolyte solution.
9. The preparation method according to claim 8, characterized in that: The electrochemical deposition method adopts constant current, constant potential or pulse electrodeposition, preferably constant current; the power consumed per square centimeter of electrode surface is 8 to 12C.
10. The preparation method according to claim 4, characterized in that: The three-dimensional flexible substrate is a substrate that has been activated by an activator, and the activator is one of sulfuric acid, nitric acid, phosphoric acid, potassium hydroxide, potassium carbonate, and zinc chloride; the activation treatment temperature is 80-160° C. and the time is 4-8 hours.
Citation Information
Patent Citations
Preparation method of titanium-based PbO2 anode with conductive ceramic membrane intermediate layer based on in-situ thermal reaction
CN110820030A
Preparation method of LPFG for detecting pH value
CN114199824A
All-solid-state pH sensor based on hydrogen storage alloy
CN117092179A
Molecularly imprinted electrochemical sensor for detecting dopamine based on titanium carbide / MOF-5 derived carbon and detection method thereof