GMR magnetic sensor manufacturing method and annealing device
Through magnetron sputtering technology and current spin orbital torque regulation, Wheatstone full-bridge structure is formed, combined with magnetic annealing furnace and thermally insulated spoiler device, the problems of regulation accuracy and annealing efficiency in GMR magnetic sensor manufacturing are solved, and high efficiency is achieved , safe production of magnetic sensors.
Patent Information
- Application Number
- CN202410815610.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing GMR magnetic sensor manufacturing methods, the regulation methods are old, errors are prone to decrease accuracy, low preparation efficiency, and uneven nitrogen distribution during the annealing process affects electrical performance, increasing safety risks and production time.
The GMR multi-layer film structure is grown using magnetron sputtering technology, and the spin orbital moment of current is used to regulate the magnetization direction of the pinned layer, and magnetization is formed in combination with a magnetic annealing furnace to achieve the regulation of the Wheatstone full-bridge structure and heat insulation is used. The spoiler ensures that the nitrogen is evenly distributed.
It improves the integration and growth efficiency of GMR magnetic sensors, reduces regulation costs and energy consumption, achieves a more efficient annealing process, and enhances safety and electrical performance.
Smart Images

Figure CN118962208A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of GMR magnetic sensor manufacturing, and in particular to a GMR magnetic sensor manufacturing method and an annealing device. Background Art
[0002] With the rapid development of information technology and the rise of concepts such as smart cities and the Internet of Things, people have put forward higher requirements for the application of sensors. Among them, magnetic sensors have been widely used in important fields such as biomedicine, industry, and navigation. Giant magnetoresistance (GMR) sensors are the leaders among many magnetic sensors, with the advantages of high detection sensitivity and easy integration.
[0003] In order for the GMR sensor to have practical value, the industry needs to design it into a Wheatstone full-bridge structure. To obtain better performance output, the free layer magnetization is parallel (or anti-parallel) and the magnetization direction of the pinned layer of the adjacent magnetoresistive unit is anti-parallel, and the magnetization directions of the free layer and the pinned layer are kept orthogonal. In order to obtain a Wheatstone structure GMR with such a magnetization direction relationship, the current control methods are relatively old:
[0004] One method is to grow the same magnetoresistive units, cut the magnetoresistive devices, and assemble them according to the requirements of the Wheatstone bridge structure. This method can perform performance testing and selection on the magnetoresistive units on the bridge arms, but errors are prone to occur in the later assembly process, resulting in problems such as reduced sensor accuracy.
[0005] The second method is to arrange different magnetic field conditions for the four devices during the device preparation process to induce the formation of the magnetization angle relationship between the free layer and the pinned layer of each magnetoresistive unit during the growth process. However, this method has multiple steps of lithography, sputtering and other cycles, and the process is very cumbersome, which reduces the preparation efficiency of the sensor device;
[0006] At the same time, when the sensor is annealed by magnetic annealing, the material is directly placed on the workpiece platform for annealing. However, since the material is not restricted during heat treatment, it is easy to deform. In addition, due to pressure problems during heat treatment, it will not be filled too full, which will cause uneven nitrogen distribution. Uneven nitrogen distribution will cause the following problems:
[0007] If nitrogen is used as a carrier gas and its distribution is uneven, it may affect the uniform heating during the annealing process, thereby affecting the electrical properties;
[0008] Can form flammable or explosive mixtures in certain areas, increasing safety risks;
[0009] This means that more time and energy are required to achieve the desired annealing effect, reducing production efficiency. Summary of the invention
[0010] In view of the problems existing in the above-mentioned conventional GMR magnetic sensor manufacturing method and annealing device, the present invention is proposed.
[0011] Therefore, an object of the present invention is to provide a GMR magnetic sensor manufacturing method and an annealing device.
[0012] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for manufacturing a GMR magnetic sensor, comprising:
[0013] Select the substrate,
[0014] Circuit patterning, using lift-off technology to pattern the GMR multilayer film structure to form a Wheatstone full-bridge circuit;
[0015] Deposition, on the substrate, an adhesion layer, a pinning layer, a pinned layer, a non-magnetic metal layer, a free layer and a protective layer are sequentially grown by magnetron sputtering technology, and four groups of GMR multilayer film structures are obtained after debonding;
[0016] Annealing, using a magnetic annealing furnace to form magnetization in the direction of the long axis of the magnetic resistance;
[0017] Exchange bias, using the spin-orbit moment of the current to control the exchange bias direction of the pinned layer;
[0018] In the Wheatstone full-bridge structure, the exchange bias control treatment is performed on the four groups of GMR multilayer film structures by changing the current input direction, so that the magnetic resistance on the two adjacent bridge arms changes oppositely with the external magnetic field, and a GMR magnetic sensor with a full-bridge structure is obtained.
[0019] As a preferred solution of the GMR magnetic sensor manufacturing method described in the present invention, when the exchange bias is regulated by the current SOT, the current direction of the first group R1 and the third group R3 in the four groups of GMR multilayer film structures is the same, the current direction of the second group R2 and the fourth group R4 is the same, and the current flow direction is opposite to the current direction of regulating R1 and R3.
[0020] Specifically, the angle layout of the four bridge arms (see the attached manual) Figure 1 As shown in the figure, in order to obtain good output performance, sensitivity, linearity, etc., usually the adjacent bridge arms have opposite output responses to the same magnetic field. The magnetization of the pinned layers of R1 and R3 is adjusted to be vertically downward, and a current pulse of a certain length of time is passed from b to a and from c to d, respectively. While R2 and R4 are respectively passed from b to c and from d to e, the magnetization direction of the pinned layers of the two is adjusted to be vertically upward;
[0021] Compared with the traditional magnetic control method, this control method can realize magnetization control under the condition of zero magnetic field. Before control, the a and e ends should be kept disconnected to prevent the control effect from being affected by the series-parallel problem when the current pulse control is applied. After the magnetic resistance control of each bridge arm is completed, the a and e ends should be connected. When the Wheatstone full bridge is working, the non-adjacent endpoints of a (e), b, c, and d can be combined as a drive input interface or as a signal output port; when a half-bridge sensor output is required, taking R1 and R2 as an example, the a and c ends are used as the drive voltage input ports, and the voltage between ab or bc can be used as the output signal of the half-bridge structure;
[0022] As a preferred solution of the GMR magnetic sensor manufacturing method of the present invention, the free layer adopts a dual soft magnetic structure of CoFe or NiFe, and the thickness is 5nm to 20nm.
[0023] As a preferred solution of the GMR magnetic sensor manufacturing method of the present invention, the pinned layer is an antiferromagnetic layer, such as IrMn, FeMn and other antiferromagnetic alloys that can convert weak spin currents; the antiferromagnetic layer is made of IrMn or FeMn material and has a thickness of 4nm to 6nm;
[0024] The pinned layer is made of NiFe or CoFe soft magnetic material with a thickness of 2nm to 8nm;
[0025] As a preferred solution of the GMR magnetic sensor manufacturing method of the present invention, the protective layer has a thickness of 2nm to 20nm and is made of Pt heavy metal material;
[0026] As a preferred solution of the GMR magnetic sensor manufacturing method of the present invention, the non-magnetic metal layer is made of a double layer of Cu and Pt, and has a thickness of 2nm to 5nm.
[0027] Beneficial effects of the present invention: The present invention utilizes the SOT effect of some heterojunctions and heavy metals. When current passes through the material, electron flows with the same spin polarization direction are simultaneously generated on both sides. The spin electron flow reaching a certain current density can realize the regulation of the direction of the magnetic moment, independently regulate the magnetoresistance sensitivity direction of each bridge arm, and finally realize the linear voltage output of the Wheatstone bridge structure.
[0028] Since the magnetic resistance on the bridge arm can be independently controlled, the GMR sensor can be placed on a substrate, which greatly increases the integration and growth efficiency of the sensor. At the same time, no external magnetic field is required during the control process, which greatly reduces the cost of GMR sensor control, improves the efficiency of control, and eliminates the energy consumption of the magnetic field.
[0029] In order to solve the above technical problems, the present invention provides the following technical solutions: an annealing device for annealing the above GMR magnetic sensor, the annealing device comprising:
[0030] Base;
[0031] A magnetic annealing furnace body is slidably disposed on the upper surface of the base;
[0032] The tailstock part is fixed to one end of the upper surface of the base;
[0033] The heat-insulating spoiler part is arranged on one side of the tailstock part to isolate the heat during annealing;
[0034] The placing table part is installed on one side of the tailstock part and is used to place the objects to be annealed.
[0035] As a preferred solution of the annealing device described in the present invention, the tailstock part includes a fixed seat, a hollow tube is fixed at one end of the fixed seat, an air pipe is arranged at a position above the hollow tube on one side of the fixed seat, and a vacuum tube is arranged at a position on one side of the hollow tube on one side of the fixed seat.
[0036] As a preferred embodiment of the annealing device of the present invention, the heat-insulating spoiler portion comprises a heat-insulating plate, a water cavity is provided inside the heat-insulating plate, and water collecting cavities are provided at both ends of the water cavity inside the heat-insulating plate, and a water inlet pipe and a water return pipe respectively connected to the two water collecting cavities are provided on one side of the heat-insulating plate;
[0037] A spoiler is also installed in the water collecting chamber located below;
[0038] The spoiler comprises a water wheel rotatably connected to the water collecting chamber, the rotating shaft of the water wheel passes through the heat insulation plate and is equipped with spoiler blades.
[0039] As a preferred solution of the annealing device of the present invention, the placing table part includes a placing table, a connecting column is fixed on one side of the placing table, and a working area is opened on the upper surface of the placing table, and a vent hole 1 is opened through the surface of the working area;
[0040] A cover plate is arranged above the placing table, and the placing table and the cover plate are connected via a rotating follow-up assembly, and air holes 2 are provided at positions on the upper surface of the cover plate corresponding to the working area;
[0041] The rotating follow-up assembly includes a bottom column, which is fixed to the outer side of the placement table through a connecting block 1, and a guide suspension platform is arranged on the outer periphery of the bottom column, an upper column is arranged above the bottom column, and a connecting column inserted into the bottom column is fixed at the bottom of the upper column, and the upper column is fixedly installed to the outer side of the cover plate through a connecting block 2.
[0042] Beneficial effects of the present invention: The present invention can make the nitrogen distribution more uniform through the heat insulation spoiler part, which can increase the heating rate, improve the annealing efficiency and electrical performance, and avoid the formation of flammable or explosive mixtures in certain areas, thereby increasing safety protection;
[0043] The placing table part presses the annealing objects to avoid deformation caused by high temperature and improves the annealing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them:
[0045] Figure 1 The figure is a schematic diagram showing the relationship between the magnetization directions of the free layer (FL) and the pinned layer (PL) when a unidirectional magnetic field is applied to induce the magnetization direction in the magnetic annealing in the GMR magnetic sensor manufacturing method of the present invention.
[0046] Figure 2 It is a schematic diagram of the direction of the spin current generated by the heavy metal material in the GMR magnetic sensor manufacturing method of the present invention.
[0047] Figure 3 Schematic diagram of a single bridge arm control method in the GMR magnetic sensor manufacturing method of the present invention.
[0048] Figure 4 It is a schematic diagram of the relationship of the magnetization directions of the GMR finished magnetic sensor after the current pulse independently controls each magnetoresistive unit in the GMR magnetic sensor manufacturing method of the present invention.
[0049] Figure 5 It is a schematic structural diagram of the annealing device of the present invention.
[0050] Figure 6 It is a schematic structural diagram of the tailstock part in the annealing device of the present invention.
[0051] Figure 7 It is a schematic structural diagram of the heat insulation and turbulence part in the annealing device of the present invention.
[0052] Figure 8 It is a schematic structural diagram of the placement table part in the annealing device of the present invention.
[0053] Fig. 9 It is a schematic structural diagram of the rotating follow-up component in the annealing device of the present invention. DETAILED DESCRIPTION
[0054] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings.
[0055] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0056] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0057] Secondly, the present invention is described in detail with reference to the schematic diagram. When describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.
[0058] Example 1
[0059] Reference Figure 1 , provides a GMR magnetic sensor manufacturing method and an overall structural schematic diagram of an annealing device, such as Figure 1-4 , a GMR magnetic sensor manufacturing method, comprising:
[0060] Choose a substrate, such as silicon wafer, glass wafer, Kapton or PET, and clean it with acetone, alcohol and purified water before use;
[0061] Circuit patterning, using lift-off technology on GMR
[0062] Annealing, using a magnetic annealing furnace to form magnetization in the long axis direction of the magnetoresistive strip, the magnetic annealing furnace is heated at 200°C in a vacuum for 30 minutes under a magnetic field of 1000Oe to induce the formation of bias, and the magnetization direction of the free layer and the pinned layer finally obtained is along the long axis direction of the magnetoresistive strip (the magnetization direction is as shown in the attached manual Figure 1 shown);
[0063] Exchange bias, using the spin-orbit moment of the current to regulate the exchange bias direction of the pinned layer, the spin-orbit moment is used to regulate the exchange bias in the magnetoresistance, and the spin current generated by the spin Hall effect in the heavy metal layer and the (REE) effect at the heterojunction interface is controlled, as shown in the attached manual Figure 2As shown in the figure, the bottom adhesion layer is Ta. In fact, Ta is used as a heavy metal to provide spin current for exchange bias. Although the spin Hall angle of Ta is opposite to that of the pinned layer material IrMn, Ta has a larger spin Hall angle. At the same time, appropriately thickened Ta has a stronger current shunting ability and can have a stronger spin current relative to the pinned layer. Therefore, in general, the spin current of Ta can play a decisive role in the regulation of exchange bias. When a sufficiently large current flows through the multilayer film, the adhesion layer produces spins that flow inward and upward, pass through the pinned layer to reach the interface where the exchange bias is located, and regulate the direction of the exchange bias.
[0064] It should be noted that the magnetic field does not need to assist the magnetization reversal during the regulation process. The current density of the pinned layer for regulating the magnetoresistance is between 1010A m-2 and 1012A m-2. The specific current density varies depending on the ambient temperature of the regulation and the thermal conductivity of the substrate material used.
[0065] In the Wheatstone full-bridge structure, the exchange bias control treatment is performed on the four groups of GMR multilayer film structures by changing the current input direction, so that the magnetic resistance on the two adjacent bridge arms changes oppositely with the external magnetic field, and a GMR magnetic sensor with a full-bridge structure is obtained.
[0066] Furthermore, when the exchange bias is regulated by the current SOT, the current directions of the first group R1 and the third group R3 in the four groups of GMR multilayer film structures are the same, and the current directions of the second group R2 and the fourth group R4 are the same, and the current flow direction is opposite to the current direction of regulating R1 and R3. After regulation, the exchange bias pinning directions on the four groups of bridge arms are as follows: Figure 4 shown.
[0067] Furthermore, the free layer adopts a dual soft magnetic structure of CoFe or NiFe, and has a thickness of 5nm to 20nm.
[0068] Furthermore, the pinned layer is an antiferromagnetic layer, which is made of IrMn or FeMn material, has a thickness of 4nm to 6nm, and can convert an antiferromagnetic alloy with a weaker spin current;
[0069] The pinned layer is made of NiFe or CoFe soft magnetic material with a thickness of 2nm to 8nm;
[0070] The upper layer of the non-magnetic layer is Cu, which has excellent electrical conductivity for spin-polarized flow and can separate the magnetic layers on both sides. Its thickness is 2nm to 5nm. The lower layer is a thinner Pt of 1nm to 1.5nm, which can provide spin flow for regulating exchange bias.
[0071] Furthermore, the protective layer has a thickness of 2nm to 20nm, which provides protection against oxidation and corrosion. The Pt heavy metal material can not only enhance the adhesion between the multilayer film and the substrate, but more importantly, it can provide a strong spin current to improve the control efficiency. The current shunt and control effect are comprehensively considered. Because the spin current generated by Pt is opposite to the Ta spin Hall angle, it can offset the spin current generated by the bottom control pinned layer, and prevent the strong spin current generated when the exchange bias direction of the pinned layer is controlled to affect the magnetization direction of the free layer. However, it should be noted that if the thickness of the free layer and the pinned layer is too thick, the resistance will be too small and the current will be diverted, reducing the current density flowing through the middle non-magnetic layer, resulting in a decrease in the GMR rate. In addition, the thickness should be adjusted according to the actual situation considering the performance parameters of the control device (current source) to prevent the thickness from being too thick and the current density from being too small, which will affect the effect of controlling the magnetic resistance strip.
[0072] Example 2
[0073] Reference Figure 5-8 , this embodiment is different from the first embodiment in that: this embodiment discloses an annealing device, including the above-mentioned GMR magnetic sensor, and further including:
[0074] Base 100;
[0075] The magnetic annealing furnace body 200 is slidably arranged on the upper surface of the base 100, a guide rod slide is installed on the base 100, a sliding sleeve is fixed to the bottom of the magnetic annealing furnace body 200, and the sliding sleeve is sleeved on the guide rod of the guide rod slide, and the sliding of the magnetic annealing furnace body 200 can be achieved by pulling;
[0076] The tailstock portion 300 is fixed to one end of the upper surface of the base 100;
[0077] The placing table part 500 is installed at one side of the tailstock part 300 and is used for placing the objects to be annealed.
[0078] The heat-insulating spoiler part 400 is disposed on one side of the tailstock part 300 to isolate the heat during annealing;
[0079] Furthermore, the tail seat part 300 includes a fixed seat 301, a hollow tube 302 is fixed at one end of the fixed seat 301, an air pipe 303 is provided on one side of the fixed seat 301 above the hollow tube 302, and a vacuum tube 304 is provided on one side of the fixed seat 301 at one side of the hollow tube 302.
[0080] Specifically, one end of the gas pipe 303 is connected to a nitrogen bottle for adding nitrogen protection during annealing;
[0081] Specifically, the other end of the vacuum tube 304 is connected to a vacuum device for extracting impurity gases in the annealing chamber;
[0082] Specifically, a thermocouple is installed in the hollow tube 302, and a through hole 1 connected to the hollow tube 302 is opened on one side of the fixing seat 301. An electrode seat is installed on the through hole 1 for connecting the thermocouple, and the thermocouple is used to monitor the internal temperature during annealing;
[0083] Furthermore, the heat-insulating spoiler part 400 includes a heat-insulating plate 401, a water cavity 402 is provided inside the heat-insulating plate 401, and water collecting cavities 403 are provided inside the heat-insulating plate 401 at both ends of the water cavity 402, and a water inlet pipe 404 and a water return pipe 405 are provided on one side of the heat-insulating plate 401, which are connected to the two water collecting cavities 403 respectively;
[0084] The water inlet pipe 404 is connected to the external water source to transport water into the water collecting chamber 403, and the water is then transported through the water chamber 402. The water transported in the water chamber 402 will heat the temperature of the insulation plate 401 to prevent high temperature from entering the fixed seat 301 and damaging the electrical components on the fixed seat 301.
[0085] Specifically, through holes are provided on the surface of the heat-insulating plate 401 at positions corresponding to the hollow tube 302, the air tube 303, and the vacuum tube 304, for the hollow tube 302, the air tube 303, and the vacuum tube 304 to pass through;
[0086] Specifically, a spoiler 406 is also installed in the water collecting chamber 403 located at the bottom;
[0087] Specifically, the spoiler 406 includes a water wheel 406a rotatably connected to the water collecting chamber 403. The rotating shaft of the water wheel 406a passes through the insulation disk 401 and is equipped with a spoiler blade 406b. The spoiler blade 406b is composed of five willow blades. The air flow generated during rotation is relatively large, which improves the uniform distribution of nitrogen in the annealing chamber. On the one hand, it increases the heat absorption rate and improves the annealing efficiency and electrical performance. On the other hand, it can avoid the formation of flammable or explosive mixtures in certain areas, thereby increasing safety protection.
[0088] Specifically, the water cavity 402 is an arc-shaped structure, which plays the role of diversion acceleration when water flows through, increases the speed of the water flow, and increases the impact on the water wheel 406a. The lower end of the water cavity 402 is connected to the bottom water collection cavity 403 at one o'clock, just located at the upper left of the water wheel 406a, and the impact angle is just conducive to the rotation of the water wheel 406a.
[0089] The rest of the structure is the same as that of Example 1.
[0090] Operation process: Place the object to be annealed on the placement table 500, and pull the magnetic annealing furnace body 200 until it fits with the fixing seat 301. At this time, the object to be annealed enters the annealing chamber, and the gas in the annealing chamber is extracted by the vacuum equipment;
[0091] Nitrogen is further transported into the annealing chamber as a protective gas through the air pipe 303. During annealing, the water inlet pipe 404 is connected to an external water source to transport water into the water collecting chamber 403. The water source is then transported through the water chamber 402. The water chamber 402 is an arc-shaped structure, which plays a role of diversion acceleration when water flows through, increases the speed of the water flow, and increases the impact on the water wheel 406a. The lower end of the water chamber 402 is connected to the bottom water collecting chamber 403 at one o'clock, just located at the upper left of the water wheel 406a. The impact angle is just conducive to the rotation of the water wheel 406a. After the water wheel 406a rotates, it drives the spoiler blade 406b to rotate. The air flow generated during the rotation is relatively large, which improves the uniform distribution of nitrogen in the annealing chamber. On the one hand, it increases the heat rate and improves the efficiency and electrical performance of annealing. On the other hand, it can avoid the formation of flammable or explosive mixtures in certain areas, thereby increasing safety protection.
[0092] Example 3
[0093] Reference Fig. 9 , this embodiment is different from the above embodiment in that: the placing table part 500 of this embodiment includes a placing table 501, a connecting column 502 is fixed to one side of the placing table 501, and a working area 503 is opened on the upper surface of the placing table 501, and a vent hole 504 is opened through the surface of the working area 503;
[0094] Furthermore, a cover plate 505 is provided above the placement table 501 , and the placement table 501 and the cover plate 505 are connected via a rotating follow-up component 506 , and air holes 507 are provided on the upper surface of the cover plate 505 at positions corresponding to the working area 503 .
[0095] Specifically, a plug sleeve is fixed at one end of the hollow tube 302, a rectangular hole is opened in the plug sleeve, and the connecting column 502 is a rectangular structure, which is convenient for inserting into the rectangular hole for fixing;
[0096] The objects are placed in the work area 503, and the cover plate 505 is placed on the placement table to fit the objects and prevent deformation and damage during annealing. The vent 1 504 and the vent 2 507 ensure that they can be in contact with nitrogen during pressing to prevent oxidation and improve heating.
[0097] Specifically, the rotating follow-up assembly 506 includes a bottom column 506a, which is fixed to the outer side of the placement table 501 through a connecting block 1 506b, and a guide suspension platform 506c is arranged on the outer periphery of the bottom column 506a, an upper column 506d is arranged above the bottom column 506a, and a connecting column 506e inserted into the bottom column 506a is fixed to the bottom of the upper column 506d, and the upper column 506d is fixedly installed on the outer side of the cover plate 505 through a connecting block 2 506f.
[0098] Specifically, the guide suspension 506c is spirally set on the bottom column 506a, and the guide suspension 506c is divided into a climbing section and a horizontal section. One side of the bottom connecting block 506f of the climbing section is at the same level. When opening and rotating, the upper column 506d is rotated. After the upper column 506d is rotated, the connecting block 506f will move in line with the guide suspension 506c. As the climbing section gradually rises, the upper column 506d moves upward, and at the same time drives the cover plate 505 to move upward during rotation until the connecting block 506f moves to the horizontal section of the guide suspension 506c. When closing, just rotate in the opposite direction, and gradually move downward to fit the surface of the object during rotation. This structure will not cause the cover plate 505 to scratch the object when closing, thus avoiding scratches on the object due to friction.
[0099] The rest of the structure is the same as that of Example 2.
[0100] Operation process: the object is placed in the work area 503, and the cover plate 505 is placed on the placement table to fit the object and prevent deformation and damage during annealing. The vent hole 1 504 and the vent hole 2 507 ensure that the object can be in contact with nitrogen during pressing to prevent oxidation and improve heating.
[0101] When closing the cover 505, just rotate it in the opposite direction, and gradually move downward to fit the surface of the object during rotation. This structure will not cause the cover 505 to scratch the object when closing, thus avoiding scratches on the object due to friction.
[0102] Importantly, it should be noted that the construction and arrangement of the present application shown in a plurality of different exemplary embodiments are only exemplary. Although only a few embodiments are described in detail in this disclosure, it should be readily understood by those who refer to this disclosure that many modifications are possible (e.g., the size, scale, structure, shape and proportion of various elements, and parameter values (e.g., temperature, pressure, etc.), installation arrangement, use of materials, color, directional changes, etc.) without substantially departing from the novel teachings and advantages of the subject matter described in the application. For example, the element shown as integrally formed can be composed of multiple parts or elements, the position of the element can be inverted or otherwise changed, and the nature or number or position of the discrete element can be changed or changed. Therefore, all such modifications are intended to be included in the scope of the present invention. The order or sequence of any process or method steps can be changed or reordered according to alternative embodiments. In the claims, any "device plus function" clause is intended to cover the structure of performing the function described herein, and is not only structurally equivalent but also equivalent structure. Without departing from the scope of the present invention, other replacements, modifications, changes and omissions can be made in the design, operating conditions and arrangement of the exemplary embodiments. Therefore, the invention is not limited to a specific embodiment, but extends to numerous modifications still falling within the scope of the appended claims.
[0103] Additionally, in order to provide a concise description of exemplary embodiments, all features of an actual embodiment (ie, those features that are not relevant to the best mode presently contemplated for carrying out the invention or those that are not relevant to implementing the invention) may not be described.
[0104] It will be appreciated that in the development of any actual implementation, as in any engineering or design project, numerous implementation-specific decisions may be made. Such a development effort may be complex and time-consuming, but will be a routine task of design, fabrication, and production for those of ordinary skill having the benefit of this disclosure without undue experimentation.
[0105] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A method for manufacturing a GMR magnetic sensor, characterized in that: include: Select the substrate, Circuit patterning, using lift-off technology to pattern the GMR multilayer film structure to form a Wheatstone full-bridge circuit; Deposition, on the substrate, an adhesion layer, a pinning layer, a pinned layer, a non-magnetic metal layer, a free layer and a protective layer are sequentially grown by magnetron sputtering technology, and four groups of GMR multilayer film structures are obtained after debonding; Annealing, using a magnetic annealing furnace to form magnetization in the direction of the long axis of the magnetic resistance; Exchange bias, using the spin-orbit moment of the current to control the exchange bias direction of the pinned layer; In the Wheatstone full-bridge structure, the exchange bias control treatment is performed on the four groups of GMR multilayer film structures by changing the current input direction, so that the magnetic resistance on the two adjacent bridge arms changes oppositely with the external magnetic field, and a GMR magnetic sensor with a full-bridge structure is obtained.
2. The method for manufacturing a GMR magnetic sensor according to claim 1, wherein: When the current SOT regulates the exchange bias, the current directions of the first group R1 and the third group R3 in the four groups of GMR multilayer film structures are the same, the current directions of the second group R2 and the fourth group R4 are the same, and the current flow direction is opposite to the current direction of regulating R1 and R3.
3. The method for manufacturing a GMR magnetic sensor according to claim 2, wherein: The free layer adopts a dual soft magnetic structure of CoFe or NiFe with a thickness of 5nm to 20nm.
4. The method for manufacturing a GMR magnetic sensor according to claim 3, wherein: The pinning layer is an antiferromagnetic layer, which is made of IrMn or FeMn and has a thickness of 4nm to 6nm; The pinned layer is made of NiFe or CoFe soft magnetic material with a thickness of 2nm to 8nm.
5. The method for manufacturing a GMR magnetic sensor according to claim 4, wherein: The protective layer has a thickness of 2nm to 20nm and is made of Pt heavy metal material.
6. The method for manufacturing a GMR magnetic sensor according to claim 5, wherein: The non-magnetic metal layer is made of a double layer of Cu and Pt, and has a thickness of 2nm to 5nm.
7. An annealing device, characterized in that: Used for annealing the GMR magnetic sensor according to any one of claims 1 to 6, the annealing device comprising: Base (100); A magnetic annealing furnace body (200) is slidably disposed on the upper surface of the base (100); A tailstock portion (300) is fixed to one end of the upper surface of the base (100); A heat-insulating spoiler part (400) is arranged on one side of the tailstock part (300) and is used to isolate heat during annealing; The placing table part (500) is installed on one side of the tailstock part (300) and is used for placing the objects to be annealed.
8. The annealing device according to claim 7, characterized in that: The tailstock part (300) comprises a fixed seat (301), a hollow tube (302) is fixed to one end of the fixed seat (301), an air pipe (303) is arranged at a position above the hollow tube (302) on one side of the fixed seat (301), and a vacuum tube (304) is arranged at a position on one side of the hollow tube (302) on one side of the fixed seat (301).
9. The annealing device according to claim 8, characterized in that: The heat-insulating spoiler portion (400) comprises a heat-insulating plate (401), a water cavity (402) is provided inside the heat-insulating plate (401), and water collecting cavities (403) are provided inside the heat-insulating plate (401) at both ends of the water cavity (402), and a water inlet pipe (404) and a water return pipe (405) respectively connected to the two water collecting cavities (403) are provided on one side of the heat-insulating plate (401).
10. The annealing device according to claim 9, characterized in that: The placing table part (500) comprises a placing table (501), a connecting column (502) is fixed on one side of the placing table (501), a working area (503) is provided on the upper surface of the placing table (501), and a vent hole (504) is provided through the surface of the working area (503); A cover plate (505) is arranged above the placement platform (501), and the placement platform (501) and the cover plate (505) are connected via a rotating follow-up component (506), and a second air vent (507) is provided on the upper surface of the cover plate (505) at a position corresponding to the working area (503).