Lead frame surface coarsening method and coarsened lead frame

Through the coordinated method of laser ablation and sodium persulfate solution, the surface of the lead frame is accurately roughened, which solves the problems of high cost, long cycle and environmental pollution in the production process of the lead frame, and achieves efficient and environmentally friendly surface roughening treatment. , improves the reliability of packaged devices.

CN118969630APending Publication Date: 2024-11-15ZHENGZHOU XINGHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034047.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There are problems of high cost, long cycle, poor conversion and environmental pollution in the production process of existing lead frames.

Method used

The surface of the lead frame is accurately roughened by laser ablation and sodium persulfate solution, and a microconcave-convex structure is formed by laser ablation, and chemical corrosion is used for sodium persulfate solution at room temperature to form a rough surface. Use protective agents to prevent oxidation and corrosion and reduce environmental pollution.

Benefits of technology

It realizes rapid, simple and coarse surface of the lead frame, reduces production costs, shortens processing cycles, improves the reliability and environmental protection of packaging devices, reduces environmental pollution, and ensures the integrity of the silver plating area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969630A_ABST
    Figure CN118969630A_ABST
Patent Text Reader

Abstract

The invention discloses a method for coarsening the surface of a lead frame and a coarsened lead frame, and the method comprises the steps: firstly, determining a laser ablation region, and carrying out the laser ablation of a non-silver-plated region of the to-be-coarsened lead frame; soaking the ablated lead frame in a sodium persulfate solution at room temperature; and finally, washing the obtained lead frame with water, soaking the lead frame in a protective agent, and drying the lead frame to obtain the coarsened lead frame. According to the method, through the synergistic effect of laser ablation and chemical corrosion, the binding force between the surface of the copper base material and the molding powder is remarkably improved, the reliability of a packaging device can be improved, the method has the advantages of being rapid and easy, the production cost can be reduced, and the machining period can be shortened. Meanwhile, compared with a traditional chemical corrosion method, the method has the advantages that pollution to the environment is reduced, accurate coarsening of the surface of the lead frame is achieved, meanwhile, a key plating layer is reserved, and the reliability and the environmental protection property of a packaging device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor integrated circuit packaging and testing, and relates to a method for roughening the surface of a lead frame and a roughened lead frame. Background Art

[0002] In the semiconductor plastic encapsulation industry, surface roughening of lead frames is an important technical point for encapsulating high-reliability plastic encapsulated devices. There are tiny pores on the surface of the roughened lead frame. Under a microscope, it can be seen that the surface is rough, porous, and enlarged, which can combine with the plastic powder for a larger surface area during the encapsulation process. The combination of more surface area means that the interface bonding strength is improved. At the same time, the rough interface increases the difficulty of external moisture intrusion into the device, thereby improving the reliability and moisture absorption sensitivity of the plastic encapsulated device. Based on this mechanism and advantage, lead frames with roughened surfaces have been widely used in the encapsulation of plastic encapsulated devices in the military, automotive and other fields.

[0003] At present, the industry generally performs surface roughening treatment on lead frames during lead frame production. Lead frame manufacturers perform roughening treatment on specific or all areas according to the needs of packaging manufacturers. Currently, micro-etching roughening method and browning roughening method are mainly adopted. The specific technology of micro-etching roughening method is: (1) preparing the copper substrate of the lead frame by stamping or etching; (2) using professional chemical solution to perform micro-chemical corrosion reaction on the copper substrate of the lead frame, usually by spraying; (3) cleaning the copper substrate of the lead frame after the micro-chemical corrosion reaction to form a lead frame with roughening characteristics. In order to further increase the roughening effect of the copper substrate, some lead frame manufacturers plate a thin layer of copper on the copper substrate after cleaning; (4) selectively silver-plating is performed on the roughened copper substrate of the lead frame under the cover of the electroplating silver template. After silver plating, the roughened lead frame production is completed. The specific technology of the browning roughening method is as follows: (1) Prepare the lead frame copper substrate by stamping or etching; (2) Use professional chemical solution to oxidize or organically treat the surface of the lead frame copper substrate to form a rough surface structure on the copper material surface, and at the same time form a thin oxide layer or organic layer, and enhance the bonding force between the lead frame and the plastic powder through the physical latch structure and chemical bond force; (3) Clean the oxidized or organically treated lead frame copper substrate; (4) Under the cover of the electroplating silver template, selective silver plating is performed on the roughened lead frame copper substrate, and the roughened lead frame is produced after silver plating. The main difference between the micro-etching roughening method and the browning roughening method is the choice of roughening solution, which makes the surface roughening effect of the copper substrate different.

[0004] The main problems with the above technical methods are: (1) high cost. Lead frame manufacturers need to configure special spraying equipment to spray chemicals to produce a roughened surface, and they also need to add special chemical solutions; (2) long cycle. The application field of roughened lead frames is special, with large batches and small processing quantities. Lead frame manufacturers are not willing to process them. Compared with non-roughened lead frames, the processing process is long, resulting in a longer processing cycle; (3) poor conversion. It is not easy to quickly convert non-roughened frames of the same specifications and sizes into roughened lead frames; (4) environmental pollution. Roughening requires special chemical spraying, which will inevitably increase wastewater and exhaust emissions, causing certain impacts on the ecological environment. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a method for roughening the surface of a lead frame and a roughened lead frame, thereby solving the technical problems of high cost, long cycle, poor conversion and environmental pollution in the production process of the roughened lead frame in the prior art.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for roughening the surface of a lead frame comprises the following steps:

[0008] S1: Determine the laser ablation area and perform laser ablation on the non-silver-plated area of ​​the lead frame to be roughened;

[0009] S2: soaking the ablated lead frame in a sodium persulfate solution at room temperature;

[0010] S3: After washing the lead frame obtained in step S2, immersing it in a protective agent, and drying it, a roughened lead frame is obtained.

[0011] Preferably, at least two visual reference points are set on the lead frame to be roughened, and the laser ablation area is determined using a visual recognition system of the laser device.

[0012] Preferably, the laser ablation area extends to 100um to 300um outside the plastic package.

[0013] Preferably, the laser ablated area extends to the inner side of the lead frame connecting rib.

[0014] Preferably, during the laser ablation process, the laser wavelength is 1064 nm, the ablation power is 10-30 W, and the ablation rate is 1500-2500 mm / s.

[0015] Preferably, the concentration of the sodium persulfate is 80 to 120 g / L, and the sample is immersed in the sodium persulfate solution for 1 to 5 minutes.

[0016] Preferably, in step S3, running water is used for 20s to 80s to complete the water washing process.

[0017] Preferably, in step S3, the volume concentration of the protective agent is 20% to 40%, and the sample is immersed in the protective agent for 20s to 60s.

[0018] A roughened lead frame is obtained by roughening through the above method.

[0019] Preferably, the roughness of the roughened lead frame surface is 2 um to 8 um.

[0020] Compared with the prior art, the present invention has the following beneficial technical effects:

[0021] The present invention discloses a method for roughening the surface of a lead frame. First, a laser ablation area is determined, and a non-silver-plated area of ​​the lead frame to be roughened is laser ablated. The laser ablation technology allows very precise control of the area to be roughened, avoiding damage to the silver-plated area (usually a key area for bonding in a packaging process). Laser ablation can produce a microscopic concave-convex structure on the surface of a copper substrate, which helps to improve the reactivity with chemical reagents during subsequent treatment, thereby making it easier to form a rough surface. Retaining the silver-plated area is crucial to ensuring the reliability and quality of the packaging process, and the laser ablation technology can effectively achieve this goal. Then, at room temperature, the lead frame after the ablation treatment is immersed in a sodium persulfate solution. The sodium persulfate solution can react chemically with the copper substrate to further corrode and roughen the surface after laser ablation to form a rougher structure. Operating at room temperature is conducive to reducing energy consumption and equipment costs, and also helps to maintain the stability and controllability of the treatment process. The lead frame treated with sodium persulfate is washed with water, placed in a protective agent for immersion treatment, and dried to obtain a roughened lead frame. The washing step can remove residual sodium persulfate and other impurities on the surface of the lead frame to ensure the purity of subsequent treatment. The protective agent immersion treatment can form a protective film on the surface of the roughened copper substrate to prevent it from being further oxidized or corroded, and also helps to improve the bonding force with the plastic powder. The drying process solidifies the protective agent on the surface of the copper substrate, enhances the protective effect, and ensures the dry state of the lead frame to prepare for the subsequent packaging process. The present invention significantly improves the bonding force between the copper substrate surface and the plastic powder through the synergistic effect of laser ablation and chemical corrosion, which helps to improve the reliability of the packaged device. The method has the characteristics of fastness and simplicity, can reduce production costs and shorten the processing cycle. At the same time, compared with the traditional chemical corrosion method, this method reduces pollution to the environment. The method realizes precise roughening of the lead frame surface, while retaining the key coating, and improves the reliability and environmental protection of the packaged device.

[0022] Furthermore, at least two visual reference points are set on the lead frame to be roughened, and the laser ablation is determined by the visual recognition system of the laser equipment. By identifying the preset visual reference points through the visual recognition system, the starting position and boundary of the laser ablation can be accurately determined, avoiding errors that may be caused by manual positioning. Accurate laser ablation can ensure that roughening is only performed on the non-silver-plated area, protecting the silver-plated area from damage, thereby improving the product qualification rate and reducing the scrap rate. The integration of the visual recognition system and the laser equipment realizes fully automated operation from positioning to ablation, reduces manual intervention, and improves production efficiency. Automated operation reduces the errors and uncertainties caused by manual operation and ensures the stability and consistency of the production process. By setting multiple visual reference points, the system can adapt to lead frames of different specifications and shapes without the need for a lot of adjustments to the equipment.

[0023] Furthermore, the laser ablation area extends 100um to 300um outside the plastic package, and the rough surface formed by laser ablation extends 100um to 300um outside the plastic package, which effectively increases the contact area between the plastic package and the lead frame. This increased contact area provides more physical bite points, thereby enhancing the bonding force between the two. Closer contact helps to reduce the gap between the plastic package and the lead frame, improve the sealing of the packaged device, and prevent the intrusion of external moisture and other harmful substances. The epitaxy of the laser ablation area increases the heat dissipation area of ​​the lead frame to a certain extent. During the operation of the packaged device, the heat generated can be dissipated through a wider area, which helps to reduce the operating temperature of the device and improve the stability and reliability of the device. The rough surface structure may help to improve the thermal conductivity, so that heat can be transferred to the outside of the package more quickly, further reducing the temperature gradient inside the device. By adjusting the epitaxial size (100um to 300um) of the laser ablation area, it can adapt to the needs of different packaging processes and device designs. This flexibility helps to meet the performance requirements in different application scenarios. During the packaging process, the difference in thermal expansion coefficient between the plastic package and the lead frame may lead to stress concentration and cracks. The epitaxy of the laser ablation area helps to disperse these stresses and reduce the risk of cracks. The rough surface structure helps to improve the impact resistance of the packaged device. When subjected to external impact, the rough surface can provide better energy absorption and dispersion effects, protecting the internal structure of the device from damage.

[0024] Furthermore, the laser ablation area extends to the inner side of the lead frame connecting ribs, and the rough surface formed by laser ablation on the inner side of the connecting ribs can increase the contact area between the plastic package and the lead frame, thereby enhancing the bonding force between them. This enhanced bonding force helps to reduce the problems of delamination and cracking during the packaging process, and improves the reliability of the packaged device. During the packaging process, due to the difference in thermal expansion coefficients between the plastic package and the lead frame, stress concentration may occur. Extending the laser ablation area to the inner side of the connecting ribs helps to form a more uniform stress distribution at the connecting ribs, reduce stress concentration, and reduce the risk of cracks. As a part of the lead frame, the connecting ribs also bear the function of heat dissipation. Extending the laser ablation area to the inner side of the connecting ribs can increase the surface area of ​​the heat dissipation path, which is conducive to the rapid transfer and dissipation of heat, thereby improving the heat dissipation performance of the packaged device. The rough surface structure helps to improve the thermal conductivity, so that heat can be more efficiently transferred to the outside of the package through the connecting ribs, further reducing the temperature gradient inside the device.

[0025] Furthermore, during the laser ablation process, the laser wavelength is 1064nm, the ablation power is 10-30w, the ablation rate is 1500-2500mm / s, and the penetration depth of the 1064nm wavelength laser can reach 5-10mm. The deeper penetration depth means that the laser energy can act more effectively on the deep layer of the target material, thereby achieving a more thorough ablation effect. Since the wavelength of the 1064nm laser is longer, its heat diffusion area is relatively small, which helps to reduce the thermal damage to the surrounding tissue during the ablation process and improve the processing accuracy. Adjusting the ablation power within the range of 10-30W can be precisely controlled according to the specific material and processing requirements. The lower power is suitable for fine processing, while the higher power is suitable for rapid removal of a large amount of material. Appropriate power setting can reduce the thermal effect during laser ablation, reduce thermal damage to surrounding tissues, and protect non-processing areas. Under the premise of ensuring processing quality, increasing the ablation power can speed up the processing speed and improve production efficiency. A higher ablation rate means a faster processing speed, which helps to shorten the production cycle and improve production efficiency. The fast ablation process can reduce the laser's residence time on the target material, thereby reducing the heat accumulation effect and reducing thermal damage to the material. The appropriate ablation rate can ensure the uniform distribution of laser energy on the target material and improve the flatness and consistency of the processed surface. This setting achieves fine control of the laser ablation process by precisely controlling the laser wavelength, ablation power and ablation rate, ensuring processing quality and efficiency.

[0026] Furthermore, the concentration of the sodium persulfate is 80 to 120 g / L, and the object is immersed in the sodium persulfate solution for 1 to 5 minutes. Sodium persulfate is a strong oxidant. Within the set concentration range, sodium persulfate can give full play to its oxidizing properties and effectively remove dirt, grease, organic residues, etc. on the surface of the object to be treated. The appropriate immersion time (1 to 5 minutes) ensures that the sodium persulfate solution can fully penetrate into the surface and tiny gaps of the object to be treated, thereby achieving a more comprehensive cleaning effect. Sodium persulfate immersion treatment can remove oxides and impurities on the surface, improve the surface finish and adhesion, and thus help improve the quality of subsequent processing.

[0027] Furthermore, in step S3, running water is used for rinsing for 20s to 80s to complete the water washing process. The running water can continuously and stably rinse the surface of the object to be treated, and effectively remove the sodium persulfate solution remaining on the surface. This continuous rinsing action ensures the thoroughness of the surface cleaning. By rinsing for a sufficiently long time (20s to 80s), the potential impact of surface residues on subsequent processing steps or the quality of the final product can be significantly reduced, thereby reducing the risk of contamination.

[0028] Further, in step S3, the volume concentration of the protective agent is 20% to 40%, and the protective agent is soaked for 20s to 60s. The volume concentration of the protective agent is set to 20% to 40%. This range can ensure that the protective agent fully exerts its protective effect during the soaking process. Too low a concentration cannot achieve the expected protective effect, while too high a concentration increases the cost and causes unnecessary damage to the surface of the object. The soaking time is set to 20s to 60s. During this period of time, the protective agent can fully penetrate into the surface of the object and tiny gaps, and form an effective protective layer with the surface of the object to prevent corrosion, oxidation and other adverse reactions that may occur during subsequent processing or storage. By setting a reasonable soaking time, the time of the entire processing flow can be shortened while ensuring the protective effect, and the production efficiency can be improved. Within the appropriate soaking time, the protective agent can be evenly distributed on the surface of the object to form a uniform protective film, which helps to ensure the stability and consistency of the processing quality and avoid quality problems caused by uneven processing. Too short a soaking time causes the protective agent to be unable to fully penetrate, leaving unprotected areas on the surface of the object; while too long a soaking time increases the processing cost and causes unnecessary waste. Therefore, reasonable soaking time setting can help reduce processing defects and improve product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 A schematic diagram of a process of a lead frame surface roughening method in the present invention;

[0031] Figure 2 This is a schematic diagram of the front side of a non-roughened lead frame;

[0032] Figure 3 This is a schematic diagram of the back side of a non-roughened lead frame;

[0033] Figure 4 Schematic diagram of laser ablation of the front side of a non-roughened lead frame in the present invention;

[0034] Figure 5 Schematic diagram of laser ablation of the back side of a non-roughened lead frame in the present invention;

[0035] Figure 6 Schematic diagram of the laser ablation effect of the lead frame copper substrate in the present invention.

[0036] Among them: 1. Lead frame, 2. Lead frame copper substrate, 3. Lead frame silver-plated area, 4. Lead frame carrier, 5. Edge of device plastic package, 6. Frame connecting ribs, 7. The first visual reference point on the front of the lead frame, 8. The second visual reference point on the front of the lead frame, 9. The first visual reference point on the back of the lead frame, 10. The second visual reference point on the back of the lead frame. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0038] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0039] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0040] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0041] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0042] like Figure 1 As shown, the present invention provides a method for roughening the surface of a lead frame, comprising the following steps:

[0043] S1: Determine the laser ablation area and perform laser ablation on the non-silver-plated area of ​​the lead frame to be roughened;

[0044] When determining the laser ablation area, at least two visual reference points are set on the lead frame to be roughened, and the laser ablation area is determined using a visual recognition system of the laser device.

[0045] Preferably, the laser ablation area extends to 100um to 300um outside the plastic package.

[0046] Further preferably, the laser ablated area extends to the inner side of the lead frame connecting rib.

[0047] During the laser ablation process, the laser wavelength is 1064nm, the ablation power is 10-30w, and the ablation rate is 1500-2500mm / s.

[0048] S2: soaking the ablated lead frame in a sodium persulfate solution at room temperature;

[0049] Wherein, the concentration of the sodium persulfate is 80-120 g / L, and the sample is immersed in the sodium persulfate solution for 1-5 minutes.

[0050] S3: After washing the lead frame obtained in step S2, immersing it in a protective agent, and drying it, a roughened lead frame is obtained.

[0051] During the water washing process, running water is used for washing for 20s to 80s to complete the water washing process.

[0052] The volume concentration of the protective agent is 20% to 40%, and the material is immersed in the protective agent for 20s to 60s.

[0053] The present invention discloses a method for roughening the surface of a package lead frame. The non-roughened lead frame is quickly transformed into a roughened oxidized frame by laser ablation and deoxidation treatment. The laser ablation effectively retains the silver-plated area used for bonding in the packaging process, and the surface roughening of the copper substrate on the front and back of the lead frame is achieved, thereby improving the bonding force between the copper substrate surface and the plastic powder in the encapsulation link, and hindering the intrusion of external moisture, thereby improving the reliability and moisture absorption sensitivity of the plastic-encapsulated device. The present invention can quickly and easily transform a non-roughened lead frame into a roughened lead frame, while reducing the production cost of the roughened lead frame, shortening the processing cycle, and reducing pollution to the environment.

[0054] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0055] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0056] Example 1

[0057] The present invention aims at the problems of high cost, long cycle, poor conversion, environmental pollution, etc. in the production process of roughened lead frame, and transfers the roughening process of lead frame from lead frame manufacturing plant to packaging plant, and uses laser equipment to selectively ablate non-roughened lead frame to form a rough metal surface, and then removes the laser ablated oxide layer through processes such as cleaning, deoxidation treatment, rinsing, drying, anti-discoloration treatment, etc. The method can flexibly realize the rapid conversion of non-roughened lead frame of the same specification size into roughened lead frame, which is suitable for small batch, multi-type high-reliability plastic package product packaging. The present invention provides a method for roughening the surface of packaged lead frame, and performs secondary processing on non-roughened lead frame before packaging process to achieve roughening of specific surface area, improve the bonding strength between frame and plastic powder and hinder the intrusion of moisture. According to the interface distribution between the front side of the lead frame and the plastic powder, the silver-plated area is avoided and the copper substrate in the interface contact area between the front side of the lead frame and the plastic powder is selected by the laser equipment used in the packaging process. The laser equipment performs laser ablation on the copper substrate in the selected area. Then, the lead frame is reversed and the copper substrate in the interface contact area between the back side of the lead frame and the plastic powder is completely laser ablated. After that, chemical deoxidation and organic protective layer anti-discoloration treatment are used to complete the processing of the roughened lead frame.

[0058] The process of the present invention is specifically as follows:

[0059] (1) Selection and positioning method of laser ablation area on the front side of non-roughened lead frame

[0060] The front side of the non-roughened lead frame is divided into a silver-plated area and a non-silver-plated area. The silver-plated area needs to be reserved for packaging process bonding, and the non-silver-plated area needs to be positioned for laser ablation.

[0061] First, the non-silver-plated area that needs to be laser ablated is selected, and the copper substrate on the front side of the lead frame that contacts the plastic powder is laser ablated as much as possible according to the principle of maximization. Figure 2As shown, the front of the lead frame 1 has a lead frame copper substrate 2, that is, a non-silver-plated copper substrate, which is mainly distributed in the epitaxial part of the lead frame carrier 4 and the lead frame silver-plated area 3, that is, the silver-plated bonding area. The lead frame carrier 4 is fully silver-plated or partially silver-plated, annularly silver-plated, etc., and the silver-plated area needs to be retained during laser ablation. The front of the frame carrier is completely encapsulated in plastic powder, and the non-silver-plated area needs to be ablated; the epitaxial part of the silver-plated bonding area is divided into the inner part of the plastic package and the outer part of the plastic package with the edge 5 of the device plastic package as the boundary, and the non-silver-plated area of ​​the inner part of the plastic package needs to be laser ablated; the non-silver-plated area of ​​the outer part of the plastic package needs to consider the error of the encapsulation bias mold, and needs to be extended outward by 100um to 300um from the edge of the device plastic package or extended to the inner side of the lead frame connecting rib 6 (if any). For the corresponding area on the front side of the non-roughened lead frame that needs laser ablation, the ablation area is demarcated on the laser ablation equipment, and the laser ablation equipment only performs laser ablation on the demarcated area when operating.

[0062] Secondly, in order to accurately align the ablation area of ​​each device frame and realize automatic recognition and determination of the ablation area by the laser equipment, the visual recognition system of the laser equipment is used to make more than two visual reference points on the front of each device frame, such as Figure 2 As shown, in this embodiment, a first visual reference point 7 on the front of the lead frame and a second visual reference point 8 on the front of the lead frame are provided. The visual reference points need to have pattern uniqueness. The laser device determines the position of the lead frame by visually identifying a specific pattern area and automatically determines the area that needs laser ablation.

[0063] The front of the non-roughened lead frame has a silver-plated area, and the surface of the copper substrate in the non-silver-plated area is flat. The frame carrier has a variety of situations such as full silver plating, partial silver plating, annular silver plating, and no silver plating. As mentioned above, when selecting the surface area of ​​the copper substrate to be laser ablated, the area should be selected as much as possible. The area should extend outward by 100um to 300um beyond the edge of the device plastic package or extend to the inside of the lead frame connecting ribs (if any). Set more than 2 visual reference points on the front of the frame, which can be selected diagonally or triangularly.

[0064] (2) Selection and positioning of the laser ablation area on the back of the non-roughened lead frame

[0065] The back of the non-roughened lead frame is usually a non-silver-plated area, and there are no special areas such as chip bonding and bonding. The surface of the lead frame copper substrate encapsulated in the plastic package needs to be completely laser ablated.

[0066] First, the laser ablation area is selected, such as Figure 3As shown, the back of the lead frame inside the plastic package needs to be completely laser ablated, with the edge of the device plastic package as the boundary; the back of the lead frame outside the plastic package also needs to consider the error of the encapsulation bias mold, and needs to be extended 100um to 300um outward from the edge of the device plastic package or to the inside of the lead frame connecting rib (if any). The ablation area is determined by demarcating the area on the laser ablation equipment, and the laser ablation equipment only performs laser ablation on the demarcated area when operating.

[0067] Secondly, the visual recognition system of the laser equipment is used again to make more than two visual reference points on the back of each device frame, such as Figure 3 As shown, in this embodiment, a first visual reference point 9 and a second visual reference point 10 are provided on the back of the lead frame. The visual reference points need to have pattern uniqueness. The laser device determines the position of the lead frame by visually identifying a specific pattern area and automatically determines the area that needs laser ablation.

[0068] There is no silver-plated area on the back of the non-roughened lead frame, and the copper substrate surface on the back is flat. As mentioned above, when selecting the copper substrate surface area to be laser ablated, the area should also be selected according to the principle of selection as much as possible. The area should extend 100um to 300um beyond the edge of the device plastic package or extend to the inside of the lead frame connecting rib (if any), corresponding to the area selected on the front. Set more than two visual reference points on the back of the frame, which can be selected diagonally or triangularly.

[0069] (3) Selection of light source, power, and rate for laser ablation of lead frame copper substrate

[0070] Common laser light sources include infrared light (wavelength 1064nm), green light (wavelength 532nm), and ultraviolet light (wavelength 350nm-400nm). From the perspective of the heat-affected zone, the heat-affected zone of infrared light is the largest, and it is more likely to produce a rough metal surface during laser ablation. At the same time, infrared lasers have the characteristics of large spot size, long focal length, and low cost. For a fixed area, its ablation efficiency is faster and the cost is lower. Therefore, the preferred laser light source of the present invention is an infrared laser device with a wavelength of 1064nm.

[0071] In terms of power selection, a power of more than 50w is too large, and grooves or notches will be ablated, and the ablation depth will reach more than 10um, which will not achieve the effect of roughening the metal surface in the area, but will reduce the thickness of the lead frame copper substrate, causing problems such as poor consistency of lead frame thickness, reduced support force, and easy warping; a power of less than 5w is too small, the ablation effect of the copper substrate surface is poor, the ablation depth is less than 1um, the effect of the rough metal surface is not obvious, the roughness is low, and the bonding force between the plastic powder and the lead frame cannot be effectively improved. Therefore, the power range of the infrared laser light source described in the present invention is 10w~30w.

[0072] In terms of laser ablation rate, too fast ablation rate leads to poor continuity of metal scars, while too slow ablation rate causes overlapping metal scars, excessive ablation depth and low efficiency. Based on engineering practice experience, the laser ablation rate is selected to be 1500mm / s to 2500mm / s.

[0073] (4) Laser ablation and deoxidation process

[0074] a. Place the front side of the non-roughened lead frame on the workbench of the laser equipment, and perform laser ablation on the front side according to the aforementioned “selection and positioning method for laser ablation area on the front side of the non-roughened lead frame” to form a Figure 4 The laser ablation area is shown. The laser light source is infrared light with a wavelength of 1064nm and an ablation power of 10w to 30w. The ablation times can be one or more times.

[0075] b. Place the back of the non-roughened lead frame on the workbench of the laser equipment, and perform laser ablation on the back area according to the aforementioned “selection and positioning method for laser ablation area on the back of the non-roughened lead frame” to form a Figure 5 The laser ablation area is shown. The laser light source is infrared light with a wavelength of 1064nm and an ablation power of 10w to 30w. The ablation times can be one or more times.

[0076] Figure 6 This is a schematic diagram of the effect of laser ablation on the lead frame copper substrate. After laser ablation, the surface of the lead frame copper substrate forms a rough metal surface as the laser spot size increases. The height difference of the surface after ablation is 2um to 8um, achieving the effect of roughening the surface of the copper substrate.

[0077] c. Place the lead frame ablated by laser in a deoxidation solution for deoxidation treatment, and rinse with pure water after deoxidation treatment. Considering that the deoxidation is mainly copper oxide and preventing the silver plating layer and copper substrate from being corroded, the deoxidation solution is sodium persulfate, and the treatment temperature is room temperature or heated.

[0078] The deoxidation mechanism here is that sodium persulfate decomposes into sodium sulfate and sulfuric acid when it meets water, and then the decomposed sulfuric acid reacts with CuO, specifically:

[0079] Na2S2O7+H2O=Na2SO4+H2SO4

[0080] CuO+H2SO4═CuSO4+H2O

[0081] d. Place the lead frame that has been deoxidized and rinsed with pure water in a protective aqueous solution at room temperature, perform anti-discoloration treatment on the lead frame, and obtain a roughened lead frame.

[0082] The protective aqueous solution, ie, the protective agent, may be benzotriazole (BTA).

[0083] Example 2

[0084] A method for roughening the surface of a lead frame comprises the following steps:

[0085] S1: Set two visual reference points on the lead frame to be roughened, and use the visual recognition system of the laser equipment to determine the laser ablation area, and laser ablate the non-silver-plated area of ​​the lead frame to be roughened; the laser ablation area extends to 100um outside the plastic package. During the laser ablation process, the laser wavelength is 1064nm, the ablation power is 10w, and the ablation rate is 1500mm / s.

[0086] S2: soaking the lead frame after the ablation treatment in a sodium persulfate solution at room temperature; wherein the concentration of the sodium persulfate is 80 g / L, and soaking in the sodium persulfate solution for 5 minutes.

[0087] S3: Rinse the lead frame obtained in step S2 with running water for 20 seconds, soak it in a protective agent, and dry it to obtain a roughened lead frame. The volume concentration of the protective agent is 20%, and the lead frame is soaked in the protective agent for 40 seconds.

[0088] Example 3

[0089] A method for roughening the surface of a lead frame comprises the following steps:

[0090] S1: Set two visual reference points on the lead frame to be roughened, and use the visual recognition system of the laser equipment to determine the laser ablation area, and laser ablate the non-silver-plated area of ​​the lead frame to be roughened; the laser ablation area extends to 300um outside the plastic package. During the laser ablation process, the laser wavelength is 1064nm, the ablation power is 30w, and the ablation rate is 2500mm / s.

[0091] S2: soaking the lead frame after the ablation treatment in a sodium persulfate solution at room temperature; wherein the concentration of the sodium persulfate is 120 g / L, and soaking in the sodium persulfate solution for 1 minute.

[0092] S3: After washing the lead frame obtained in step S2 with running water for 80 seconds, the lead frame is immersed in a protective agent and dried to obtain a roughened lead frame. The volume concentration of the protective agent is 40%, and the lead frame is immersed in the protective agent for 20 seconds.

[0093] Example 4

[0094] A method for roughening the surface of a lead frame comprises the following steps:

[0095] S1: Set two visual reference points on the lead frame to be roughened, and use the visual recognition system of the laser equipment to determine the laser ablation area, and laser ablate the non-silver-plated area of ​​the lead frame to be roughened; the laser ablation area extends to 200um outside the plastic package. During the laser ablation process, the laser wavelength is 1064nm, the ablation power is 25w, and the ablation rate is 2000mm / s.

[0096] S2: soaking the lead frame after the ablation treatment in a sodium persulfate solution at room temperature; wherein the concentration of the sodium persulfate is 100 g / L, and soaking in the sodium persulfate solution for 4 minutes.

[0097] S3: After washing the lead frame obtained in step S2 with running water for 50 seconds, immersing it in a protective agent, and drying it to obtain a roughened lead frame. The volume concentration of the protective agent is 30%, and the lead frame is immersed in the protective agent for 50 seconds.

[0098] Example 5

[0099] In order to further explain the technical solution of the present invention, it is described by the following examples:

[0100] For a 5-row, 28-column SOP8 non-roughened lead frame, the frame is 228.2952mm long and 50.8mm wide, the carrier is 90mil×90mil, the frame carrier has no silver-plated area, and the 8 inner pins have silver-plated areas. The specific implementation steps are as follows:

[0101] Step 1: Use automatic loading mode or manual mode to place the SOP8 non-roughened lead frame on the carrier of the laser equipment;

[0102] Step 2: Using the software system of the laser equipment, select a window for the lead frame of the matrix window (one window corresponds to one device package), select the lead frame area that needs laser ablation, and extend the area to the inside of the frame connecting rib;

[0103] Step 3: Use the software system of the laser equipment to set visual reference points at the upper right corner and lower left corner of the front of the selected window frame;

[0104] Step 4: Copy steps 2 and 3 to other windows on the front of the lead frame to form the selection and positioning of all areas to be laser ablated on the front of the SOP8 non-roughened lead frame, and save program 1;

[0105] Step 5: Reverse the SOP8 non-roughened lead frame, refer to steps 2, 3, and 4 to complete the selection and positioning of the area to be laser ablated on the back of the SOP8 non-roughened lead frame, and save program 2;

[0106] Step 6: After the program setting for the ablation area on the front and back of the SOP8 non-roughened lead frame is completed, select Program 1, use an infrared laser light source with a wavelength of 1064nm, set the laser ablation power to 10w, the ablation rate to 2500mm / s, and ablate 3 times to complete the laser ablation on the front of the SOP8 non-roughened lead frame;

[0107] Step 7: Select Program 2, use an infrared laser light source with a wavelength of 1064nm, set the laser ablation power to 10w, the ablation rate to 2500mm / s, and the ablation times to 3 times to complete the laser ablation on the back of the SOP8 non-roughened lead frame;

[0108] Step 8: Immerse the laser-ablated SOP8 lead frame in a sodium persulfate solution with a concentration of 80 g / L at room temperature for 5 minutes;

[0109] Step 9: Rinse the frame with pure water for 20 seconds.

[0110] Step 10: Immerse the frame in a 20% protective aqueous solution CU-1806 for 60 seconds, and then dry at 70° C. to obtain a roughened SOP8 lead frame.

[0111] Example 6

[0112] For a 2-row, 10-column LQFP44 non-roughened lead frame, the frame is 215.5mm long and 45.7mm wide, the carrier is 122mil×122mil, the frame carrier has a silver-plated area, and the 44 inner pins have a silver-plated area. The specific implementation steps are as follows:

[0113] Step 1: Use automatic loading mode or manual mode to place the LQFP44 non-roughened lead frame on the carrier of the laser equipment;

[0114] Step 2: Using the software system of the laser equipment, select a window for the lead frame of the matrix window (one window corresponds to one device package), select the lead frame area that needs laser ablation, and extend the area to the inside of the frame connecting rib;

[0115] Step 3: Use the software system of the laser equipment to set visual reference points at the upper right corner and lower left corner of the front of the selected window frame;

[0116] Step 4: Copy steps 2 and 3 to other openings on the front of the lead frame to form the selection and positioning of all areas to be laser ablated on the front of the LQFP44 non-roughened lead frame, and save program 1;

[0117] Step 5: Reverse the LQFP44 non-roughened lead frame, refer to steps 2, 3, and 4 to complete the selection and positioning of the area to be laser ablated on the back of the LQFP44 non-roughened lead frame, and save program 2;

[0118] Step 6: After the program setting for the ablation area on the front and back of the LQFP44 non-roughened lead frame is completed, select Program 1, use an infrared laser light source with a wavelength of 1064nm, set the laser ablation power to 30w, the ablation rate to 1500mm / s, and the ablation times to 2 times to complete the laser ablation on the front of the LQFP44 non-roughened lead frame;

[0119] Step 7: Select Program 2, use an infrared laser light source with a wavelength of 1064nm, set the laser ablation power to 30w, the ablation rate to 1500mm / s, and the ablation times to 2 times to complete the laser ablation on the back of the LQFP44 non-roughened lead frame;

[0120] Step 8: Immerse the laser ablated SOP8 lead frame in a sodium persulfate solution with a solubility of 120 g / L at room temperature for 1 minute;

[0121] Step 9: Rinse the frame with pure water for 80 seconds;

[0122] Step 10: Immerse the frame in a 40% protective aqueous solution CU-1806 for 20 seconds, and then dry at 70° C. to obtain a roughened LQFP44 lead frame.

[0123] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for roughening the surface of a lead frame, characterized in that: The following steps are involved: S1: Determine the laser ablation area and perform laser ablation on the non-silver-plated area of ​​the lead frame to be roughened; S2: soaking the ablated lead frame in a sodium persulfate solution at room temperature; S3: After washing the lead frame obtained in step S2, immersing it in a protective agent, and drying it, a roughened lead frame is obtained.

2. The method for roughening the surface of a lead frame according to claim 1, characterized in that: At least two visual reference points are set on the lead frame to be roughened, and the laser ablation area is determined by using the visual recognition system of the laser equipment.

3. The method for roughening the surface of a lead frame according to claim 1, characterized in that: The laser ablation area extends to 100um to 300um outside the plastic package.

4. The method for roughening the surface of a lead frame according to claim 1, characterized in that: The laser ablated area extends to the inner side of the lead frame rib.

5. The method for roughening the surface of a lead frame according to claim 1, characterized in that: During the laser ablation process, the laser wavelength is 1064nm, the ablation power is 10-30w, and the ablation rate is 1500-2500mm / s.

6. The method for roughening the surface of a lead frame according to claim 1, characterized in that: The concentration of the sodium persulfate is 80-120 g / L, and the sample is immersed in the sodium persulfate solution for 1-5 minutes.

7. The method for roughening the surface of a lead frame according to claim 1, characterized in that: In step S3, running water is used for washing for 20s to 80s to complete the washing process.

8. The method for roughening the surface of a lead frame according to claim 1, characterized in that: In step S3, the volume concentration of the protective agent is 20% to 40%, and the material is immersed in the protective agent for 20s to 60s.

9. A roughened lead frame, characterized in that: It is obtained by roughening the product according to any one of claims 1 to 8.

10. The roughened lead frame according to claim 9, characterized in that: The roughness of the roughened lead frame surface is 2um to 8um.