Primitive cell structure and process method of trench super-junction MOSFET
By using a three-layer epitaxial layer structure and multiple Al ion implantation to form a superjunction structure of P columns in SiC MOSFET, combined with a torch-shaped and separation gate structure, the on-resistance degradation and voltage withstandness of SiC MOSFET devices is solved, and high The performance optimization of withstand voltage and low on-resistance reduces process costs.
Patent Information
- Application Number
- CN202411009094.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The on-resistance and blocking capability of existing SiC MOSFET devices will degrade after long forward conduction, and the reverse recovery characteristics of the body diode are poor, resulting in current spikes and shutdown surge voltage, damaging the semiconductor device, making it difficult to be high voltage. Keep low on-resistance and high withstand voltage.
The trench superjunction MOSFET primary cell structure adopts a three-layer epitaxial layer structure, and the superjunction structure containing P columns and N columns, forms a P column through multiple Al ion implantation, and forms a gate dielectric layer of uniform thickness on the inner wall of the groove and The torch-shaped gate structure, combined with the separate gate structure, reduces the electric field of the gate oxide layer and improves the device's withstand voltage and conduction performance.
It significantly reduces the per-area ratio of SiC MOSFET, achieves higher voltage withstandability and more optimized performance, and can produce MOSFET devices of more than 600-10000V under a unified process platform, reducing the SiC MOSFET processes with different voltages. development costs.
Smart Images

Figure CN118969840A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor devices and process manufacturing, and in particular to a primitive cell structure and process method of a trench super junction MOSFET. Background Art
[0002] SiC MOSFET technology is a power semiconductor device technology based on silicon carbide material. It has excellent characteristics such as high temperature, high voltage, and high frequency, and has gradually become one of the research hotspots for the next generation of power electronic devices.
[0003] Silicon carbide has long been considered to have unique properties that make it superior to semiconductor devices formed from other commonly used semiconductor materials such as silicon (Si), gallium arsenide (GaAs) and indium phosphide (InP). Silicon carbide has a wide band gap, high melting point, low dielectric constant, high breakdown field strength, high thermal conductivity and high saturated electron drift velocity. These properties make it possible for devices made of silicon carbide to operate at higher temperatures, higher operating frequencies and higher power levels, and in some other situations where devices made of other semiconductor materials cannot operate. Silicon carbide is a disruptive technology. With the development of new energy vehicles and photovoltaic energy storage, it is replacing silicon-based technology and is beginning to receive widespread attention from the market. The process and structure of SIC MOSFET from different manufacturers are constantly improving, and product performance is also constantly improving.
[0004] When power electronic devices are running, the body diode of SiC MOSFET devices often works in the third quadrant as a freewheeling diode. Since the bandgap width of the SiC material itself is as high as 3.26eV, the turn-on voltage of the body diode of the MOSFET device is very high, which greatly increases its loss when used as a freewheeling diode. After the body diode is forward-conducted for a long time, it may cause the degradation of the on-resistance and blocking ability of the MOSFET; and because the reverse recovery characteristics of the body diode are poor, a considerable current spike and turn-off surge voltage will be generated in this process, and its conduction characteristics will be degraded, and in severe cases, the semiconductor device will be damaged. After the body diode is forward-conducted for a long time, its conduction characteristics will be degraded, and it may even cause the degradation of the on-resistance and blocking ability of the MOSFET.
[0005] The SiC power MOSFET market has expanded significantly since 2010, and many new players have entered the market, with double-digit compound annual growth rates expected as SiC replaces silicon technology in multiple markets such as automotive, photovoltaics, and railways. Typically, SiC power MOSFETs operate at 1200 or 1700V and are designed to replace IGBT technology in certain areas.
[0006] The device structure of SiC MOSFET mainly includes: channel region, source region, drain region and gate region. The channel region is composed of p-type SiC, the source region is composed of n+ type SiC, the drain region is composed of n+ doped SiC substrate and metal contact layer, and the gate region is composed of metal or Poly. Its working principle is to control the conductive characteristics of the channel region by changing the gate voltage, thereby controlling the current in the drain region.
[0007] The traditional trench SiC MOSFET original cell (pitch) structure, deep trench and Source Shield Plate electrode can deplete the high-concentration N-type region in the reverse withstand voltage process of the device, similar to the superjunction P column, so that the gate oxide layer electric field in the Gate Trench area is reduced, and the device has a lower unit area specific on-resistance (RSPA) when it is forward-conducted. For example, a 2μm deep P column formed by injection can deplete the higher-concentration N-type region between the two P columns during the reverse withstand voltage process of the device, so that the gate oxide layer electric field in the Gate Trench area is reduced, and the device has a lower unit area specific on-resistance when it is forward-conducted.
[0008] A vertical channel SiC MOSFET structure with low on-resistance and high temperature range characteristics is formed on the C-side of the silicon carbide substrate, forming an N-drift layer above the N+ substrate, followed by a P-channel layer. The trench gate penetrates the P-channel layer and forms an N+ source region. The metal source and drain electrodes are located at the top and bottom of the die, respectively. This trench architecture is sometimes called MMOS (U-shaped gate) to distinguish it from the planar DMOS (VDMOS) design.
[0009] Cree, a well-known LED lighting manufacturer, focuses on planar SiC MOSFET technology and has developed three generations of products. The latest generation will switch to a trench gate structure. Other manufacturers including Infineon, Rohm, Bosch, and Fuji use trench or MMOS technology. In contrast, STMicroelectronics also focuses on planar SiC MOSFET technology. The difference between Rohm's trench gate MOSFET structure and MMOS is that Rohm's third-generation trench SIC MOSFET uses some structural features of the vertical trench SiC MOSFET. The original cell size of Rohm's fourth-generation trench SiC MOSFET pitch structure is reduced to 2μm, and the original cell size of the BOSCH TMOS trench SiC MOSFET pitch structure is 3.3μm.
[0010] In recent years, SiC MOSFET technology has continued to develop, mainly reflected in the following aspects: 1. Improve device performance: By optimizing the process flow of SiC MOSFET and the pitch structure of the device, such as trench structure and super junction structure, the performance of SiC MOSFET, such as low leakage current, high switching speed, low on-resistance and low switching loss, is improved.
[0011] 2. Improvement of packaging technology: Packaging technology is one of the important factors affecting the performance and reliability of SiC MOSFET. At present, the commonly used SiC MOSFET packaging technologies include TO-220, TO-247, D2PAK, etc., and the latest packaging technology uses high-end technologies such as SiC substrate, silver-free solder, sintering, etc., which can effectively improve the device's working junction temperature and heat dissipation performance.
[0012] 3. Application expansion: SiC MOSFET technology has been widely used in electric vehicles, solar inverters, wind inverters, high-speed trains, power grid transmission and other fields. As technology continues to develop, SiC MOSFET will be used in more application scenarios.
[0013] The development direction of SiC MOSFET power devices is to reduce the device area as much as possible while ensuring low specific on-resistance, increase power density and reduce costs. Summary of the invention
[0014] The technical problem to be solved by the present invention is to provide a primitive cell structure of a trench super junction MOSFET, which has higher performance and a more compact primitive cell structure.
[0015] Another technical problem to be solved by the present invention is to provide a process method for the primitive cell structure of the trench super junction MOSFET.
[0016] In order to solve the above problems, a primitive cell structure of a trench super junction MOSFET described in the present invention comprises: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The sidewalls in the trench have a gate dielectric layer of uniform thickness, which electrically isolates the gate conductive material filled in the trench from the epitaxial layer; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
[0017] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 ; The epitaxial layer includes at least two epitaxial layers, namely a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the groove is located in the third epitaxial layer.
[0018] Furthermore, the epitaxial layer also includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
[0019] Furthermore, in the super junction structure, the concentration and doping concentration of the P column match the doping concentration of the epitaxial layer that forms the super junction structure with the P column, so as to achieve charge balance.
[0020] Furthermore, in the epitaxial layer, the depth of the trench is 2 to 6 μm, and the depth of the P column of the super junction structure is 2 to 6 μm.
[0021] Furthermore, the thickness of the second epitaxial layer in the epitaxial layer is 3 μm, and the doping concentration is 3e16-1e17 cm -3 The thickness of the second epitaxial layer is consistent with the implantation depth of the P column; the thickness of the third epitaxial layer is 3 μm, and the doping concentration is 1e16-1e17 cm -3 .
[0022] Furthermore, the gate dielectric layer is a thin gate oxide layer with uniform thickness, and the thickness is 350 to 1200Å.
[0023] Furthermore, the surface of the epitaxial layer also has a source metal layer, and the source metal layer is connected to the source N+ lead-out region and the P+ contact hole lead-out region through a contact hole.
[0024] The process method for manufacturing the above-mentioned trench super junction MOSFET primitive cell structure comprises the following process steps: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is subsequently used to fill the gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column of a certain depth in the epitaxial layer at the bottom of the trench; Forming a gate dielectric layer on the inner wall of the trench, filling it with a gate conductive material and etching back to form the gate of the super junction MOSFET; Photolithography and etching are performed to open the N+ injection window, and N+ ion implantation is performed to form the source N+ lead-out region of the primitive cell structure of the trench superjunction MOSFET in the P-well; photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form the P+ contact hole lead-out region of the P-well.
[0025] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 .
[0026] Furthermore, the high-energy P-type ion implantation into the epitaxial layer at the bottom of the trench to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the trench, and then multiple Al ion implantations of the P column of the super junction structure are performed; the thickness of the sacrificial oxide layer is 300 to 1000Å.
[0027] Furthermore, the hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or is metal nickel with a thickness of 2 to 3 μm.
[0028] Furthermore, the multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 KeV, the dose range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
[0029] Furthermore, the multiple Al ion implantations also include an annealing process after the implantation is completed, and the annealing conditions are 1700 degrees Celsius for 30 minutes in an argon atmosphere.
[0030] Furthermore, the ion implantation energy of the source N+ lead-out region is in the range of 40 to 90 KeV, the implantation dose is 4.5e14 to 1.0e15, and the implantation temperature is 500 degrees Celsius; the implantation conditions of the P well are adjusted according to the thickness of different gate dielectric layers and threshold requirements, and the implantation energy range is 50 to 300 KeV, and the implantation dose is 1.0e12 to 1.5e12; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, requiring that the smaller the spacing, the lower the implantation energy; the implantation energy range is 60 to 100 KeV, the implantation dose is 1.0e15, and the implantation temperature is 500 degrees Celsius.
[0031] Furthermore, the process steps further include depositing a metal layer on the surface of the epitaxial layer and etching to form a source metal, wherein the source metal is connected to the source N+ lead-out region and the P+ contact hole lead-out region.
[0032] The present invention also provides a primitive cell structure of a trench super junction MOSFET, comprising: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The trench includes the gate structure of the trench super junction MOSFET; the gate structure includes a gate and an insulating dielectric layer between the gate and the epitaxial layer; the cross section of the gate is a torch-shaped cross section morphology that is wide at the top and narrow at the bottom, a thinner gate dielectric layer is provided between the gate of the torch head at the top and the side wall of the trench, and a thicker trench field oxide layer is provided between the gate of the torch tail handle at the bottom and the side wall of the trench; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
[0033] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm-2; the epitaxial layer comprises at least two epitaxial layers, namely a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the trench is located in the third epitaxial layer.
[0034] Furthermore, the epitaxial layer also includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
[0035] Furthermore, in the super junction structure, the concentration and doping concentration of the P column match the doping concentration of the epitaxial layer that forms the super junction structure with the P column to achieve charge balance; the depth of the P column in the super junction structure is consistent with the thickness of the second epitaxial layer, so that the P column and N-type charges are balanced when the device is reversely withstand voltage, and the high-concentration N-type region is depleted while the electric field strength of the gate dielectric layer in the trench gate region is reduced.
[0036] Furthermore, in the epitaxial layer, the depth of the trench is 2 to 6 μm, and the depth of the P column of the super junction structure, that is, the thickness of the second epitaxial layer, is 2 to 6 μm.
[0037] Furthermore, the height of the gate at the upper torch-shaped head is 0.6 to 1.5 μm, and the thickness of the thinner gate dielectric layer between the gate and the trench sidewall is 350 to 1200 Å; the thickness of the thicker trench field oxide layer between the gate at the lower narrower and longer torch tail handle and the trench sidewall is 1000 to 3000 Å.
[0038] Furthermore, the gate dielectric layer is a gate oxide layer, and its formation process is a thermal oxidation process; the trench field oxide layer is formed by thermal oxidation, or a combination of deposition process and oxidation process.
[0039] Furthermore, the gate is made of polysilicon.
[0040] Furthermore, the P column is formed by merging multiple Al ion implantations with different implant energies and different implant doses at high temperature.
[0041] The process method for manufacturing the above-mentioned trench super junction MOSFET cell structure includes the following process steps: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is used for subsequent filling to form a gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column with a certain depth in the epitaxial layer at the bottom of the trench; A thicker trench field oxide layer is formed on the inner wall of the trench, a gate conductive material is filled and etched back to form a tail handle structure at the bottom of the torch-shaped gate, and then a thinner gate dielectric layer is formed on the upper part of the trench, and then the gate conductive material is continued to be filled and etched back to be flush with the surface of the epitaxial layer, so as to form a gate structure with a torch-shaped cross-section as a whole, that is, a thin gate dielectric layer is provided between the gate of the upper wider torch head and the side wall of the trench, and a thicker trench field oxide layer is provided between the gate of the lower narrow torch tail handle and the side wall of the trench; Photolithography and etching are performed to open the N+ injection window, and N+ ion implantation is performed to form the source N+ lead-out region of the primitive cell structure of the trench superjunction MOSFET in the P-well; photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form the P+ contact hole lead-out region of the P-well.
[0042] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 .
[0043] Furthermore, the epitaxial layer at least includes a second epitaxial layer and a third epitaxial layer; the second epitaxial layer contains the super junction structure of the super junction MOSFET, and the third epitaxial layer contains the gate structure of the super junction MOSFET.
[0044] Furthermore, the epitaxial layer also includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
[0045] Furthermore, the thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm-3; the thickness of the third epitaxial layer is 3μm, and the doping concentration is 1e16-1e17cm-3.
[0046] Furthermore, the thickness of the first epitaxial layer is 4 μm, and the doping concentration is 8e15-1e16 cm-3.
[0047] Furthermore, the high-energy P-type ion implantation into the epitaxial layer at the bottom of the trench to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the trench, and then multiple Al ion implantations of the P column of the super junction structure are performed; the thickness of the sacrificial oxide layer is 300 to 1000Å.
[0048] Furthermore, the hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or is metal nickel with a thickness of 2 to 3 μm.
[0049] Furthermore, the multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 Kev, the dose range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
[0050] Furthermore, the multiple Al ion implantations also include an annealing process after the implantation is completed, and the annealing conditions are 1700 degrees Celsius for 30 minutes in an argon atmosphere.
[0051] Furthermore, a thicker trench field oxide layer is formed on the inner wall of the trench, the thickness of the trench field oxide layer is 1000 to 3000Å, and after depositing the gate conductive material, it is etched back, the etching depth is 0.6 to 1.5μm from the top surface of the epitaxial layer, and the trench field oxide layer is wet etched to a thickness of 0.3μm to form a channel region, and then the gate conductive material is removed; then a gate dielectric layer with a thickness of 350 to 1200Å is formed on the inner wall of the upper part of the trench, polysilicon is deposited and etched back to form a gate with a complete structure.
[0052] Furthermore, the ion implantation energy of the source N+ lead-out region is in the range of 40 to 90 KeV, the implantation dose is 4.5e14 to 1.0e15, and the implantation temperature is 500 degrees Celsius; the implantation conditions of the P well are adjusted according to the thickness of different gate dielectric layers and threshold requirements, and the implantation energy range is 50 to 300 KeV, and the implantation dose is 1.0e12 to 1.5e12; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, requiring that the smaller the spacing, the lower the implantation energy; the implantation energy range is 60 to 100 KeV, the implantation dose is 1.0e15, and the implantation temperature is 500 degrees Celsius.
[0053] Furthermore, the process steps further include depositing a metal layer on the surface of the epitaxial layer and etching to form a source metal, wherein the source metal is connected to the source N+ lead-out region and the P+ contact hole lead-out region.
[0054] The present invention also provides a primitive cell structure of a trench super junction MOSFET, comprising: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The trench contains the gate structure of the trench super junction MOSFET; the gate structure is a separated gate structure consisting of two independent parts, upper and lower; wherein the shielding gate located at the lower part of the trench is in the shape of an elongated rod, and a thicker trench field oxide layer is provided between the shielding gate and the trench sidewall; the lateral width of the device gate located at the upper part of the trench is greater than that of the shielding gate, and the longitudinal length of the device gate is less than that of the shielding gate; and a gate dielectric layer thinner than the thickness of the trench field oxide layer is provided between the device gate and the trench sidewall; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
[0055] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm-2; the epitaxial layer comprises at least two epitaxial layers, namely a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the trench is located in the third epitaxial layer.
[0056] Furthermore, the epitaxial layer also includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
[0057] Furthermore, the thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm-3; the thickness of the third epitaxial layer is 3μm, and the doping concentration is 1e16-1e17cm-3.
[0058] Furthermore, the thickness of the first epitaxial layer is 4 μm, and the doping concentration is 8e15-1e16 cm-3.
[0059] Furthermore, the depth of the trench is 2-6 μm, and the thickness of the second epitaxial layer is consistent with the depth of the P column of the super junction structure, so that the high-concentration epitaxial layer N-type region is depleted while the electric field strength of the gate dielectric layer of the trench is reduced.
[0060] Furthermore, the P column is formed by merging multiple Al ion implantations with different implant energies and different implant doses at high temperature.
[0061] Furthermore, the longitudinal length of the device gate at the upper part of the trench is 0.6-1.5 μm, the thickness of the gate dielectric layer is 350-1200Å; the thickness of the trench field oxide layer at the periphery of the shielding gate is 1000-3000Å.
[0062] Furthermore, the device gate is the gate of the super junction MOSFET, and the shielding gate has the same potential as the source and is connected to the source through the source metal.
[0063] Furthermore, the gate dielectric layer is a gate oxide layer, and its formation process is a thermal oxidation process; the trench field oxide layer is formed by thermal oxidation, or a combination of deposition process and oxidation process.
[0064] Furthermore, the gate dielectric layer is a gate oxide layer, and the gate is made of polysilicon.
[0065] The process method for manufacturing the above-mentioned trench super junction MOSFET cell structure includes the following process steps: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is used for subsequent filling to form a gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column with a certain depth in the epitaxial layer at the bottom of the trench; A thicker trench field oxide layer is formed on the inner wall of the trench, and then a gate conductive material is deposited and filled and etched back to form a shielding gate at the bottom; then the trench field oxide layer is wet-etched to a certain thickness to form a channel region; then a thin gate dielectric layer is formed, and a gate conductive material is deposited and etched back to form a device gate; the shielding gate and the device gate formed are electrically isolated from each other; Photolithography and etching are performed to open the N+ injection window, and N+ ion implantation is performed to form the source N+ lead-out region of the primitive cell structure of the trench superjunction MOSFET in the P-well; photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form the P+ contact hole lead-out region of the P-well.
[0066] Furthermore, the semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm-2.
[0067] Furthermore, the epitaxial layer at least includes a second epitaxial layer and a third epitaxial layer; the second epitaxial layer contains the super junction structure of the super junction MOSFET, the third epitaxial layer has a groove, and the groove contains the gate structure of the separate gate structure of the super junction MOSFET.
[0068] Furthermore, the epitaxial layer also includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
[0069] Furthermore, the thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm-3; the thickness of the third epitaxial layer is 3μm, and the doping concentration is 1e16-1e17cm-3.
[0070] Furthermore, the thickness of the first epitaxial layer is 4 μm, and the doping concentration is 8e15-1e16 cm-3.
[0071] Furthermore, the width of the trench and the thickness of the trench field oxide layer or the gate dielectric layer on both sides of the trench need to match the thickness and concentration of the third epitaxial layer; the thickness of the third epitaxial layer is consistent with the depth of the trench, and the thickness of the second epitaxial layer is consistent with the depth of the P column formed by multiple high-energy injections; while the high-concentration N-type region is depleted, the electric field of the gate dielectric layer in the trench gate region is reduced.
[0072] Furthermore, the high-energy P-type ion implantation into the epitaxial layer at the bottom of the trench to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the trench, and then multiple Al ion implantations are performed to form the P column of the super junction structure; the thickness of the sacrificial oxide layer is 300 to 1000Å.
[0073] Furthermore, the hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or is metal nickel with a thickness of 2 to 3 μm.
[0074] Furthermore, the multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 KeV, the dose range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
[0075] Furthermore, after the multiple Al ion implantations to form the P columns, an annealing process is also included, and the annealing conditions are 1700° C. / 30 min in an argon atmosphere.
[0076] Furthermore, a thicker trench field oxide layer is formed on the inner wall of the trench, the thickness of the trench field oxide layer is 1000-3000Å, and after depositing the gate conductive material, it is etched back, and the etching depth is 0.6-1.5μm from the top surface of the epitaxial layer downward to form a lower shielding electrode; the trench field oxide layer is wet-etched to a thickness of 0.2-0.4μm to form a channel region; and then a gate dielectric layer with a thickness of 350-1200Å is formed on the upper inner wall of the trench, polysilicon is deposited and etched back to form the upper device gate 6.
[0077] Furthermore, the ion implantation energy of the source N+ lead-out region is in the range of 40 to 90 KeV, the implantation dose is 4.5e14 to 1.0e15 cm-2, and the implantation temperature is 500 degrees Celsius; the implantation conditions of the P well are adjusted according to the thickness of different gate dielectric layers and threshold requirements, and the implantation energy range is 50 to 300 KeV, and the implantation dose is 1.0e12 to 1.5e12 cm-2; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, requiring that the smaller the spacing, the lower the implantation energy; the implantation energy range is 60 to 100 KeV, the implantation dose is 1.0e15 cm-2, and the implantation temperature is 500°C.
[0078] Furthermore, the process steps also include depositing a metal layer on the surface of the epitaxial layer and etching to form a source metal, wherein the source metal is connected to the source N+ lead-out area and the P+ contact hole lead-out area; the source metal is also connected to the shielding electrode, so that the shielding electrode and the source have the same potential.
[0079] The original cell structure of the trench super junction MOSFET provided by the present invention combines the advantages of the trench and super junction MOSFET original cell structures, greatly reducing the specific on-resistance per unit area (RSPA) of the super junction MOSFET. Using the original cell structure and process of the present invention, MOSFET devices above 600 to 10000V can be produced under a unified SIC process platform, greatly optimizing the performance of MOSFET and reducing the cost of separate development of SiC MOSFET processes of different voltages. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] Figure 1 The present invention provides a primitive cell structure of a trench super junction MOSFET of the first structure, which has a gate dielectric layer of uniform thickness.
[0081] Figure 2 It is the primitive cell structure of the trench super junction MOSFET of the second structure provided by the present invention, and has a torch-shaped gate which is wide at the top and narrow at the bottom.
[0082] Figure 3 It is the primitive cell structure of the trench super junction MOSFET of the third structure provided by the present invention, and has a separated gate structure.
[0083] Description of Reference Numerals 1 is the N+ lead-out region (Source), 2 is the P+ contact hole lead-out region, 3 is Pwell (P well), 4 is the source metal, 5 is the gate dielectric layer, 6 is the gate, 7 is the columnar injection region, 8 is the first epitaxial layer, 9 is the second epitaxial layer, 10 is the third epitaxial layer, 11 is the substrate, 12 is the trench field oxide layer, and 13 is the source end field plate. DETAILED DESCRIPTION
[0084] The following is a specific implementation of the present invention in conjunction with the accompanying drawings, and the technical solutions in the present invention are clearly and completely described, but the present invention is not limited to the following implementations. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. According to the following description and claims, the advantages and features of the present invention will be clearer. It should be noted that the drawings are all in a very simplified form and use non-precise ratios, which are only used to conveniently and clearly assist in explaining the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0085] The present invention can be implemented in different forms and should not be interpreted as being limited to the embodiments proposed herein. On the contrary, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. In the accompanying drawings, for clarity, the size and relative size of the layers and zones may be exaggerated, and the same reference numerals represent the same elements from beginning to end. In the description of the present application, it should be noted that the orientation or positional relationship indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside", etc. is based on the orientation or positional relationship shown in the accompanying drawings, only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present application. In addition, the terms "first", "second", and "third" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0086] The embodiments of the present invention provide three types of trench superjunction MOSFET primitive cell structures, all of which use a three-layer epitaxial layer structure to achieve higher withstand voltage capability. In some cases where the withstand voltage requirement is lower than 1700V, a double-layer epitaxial layer structure can be used, that is, the first epitaxial layer 8 in the embodiments of the present invention is omitted.
[0087] The 3-layer EPI and structural parameters used in the present invention are not limited to the 1200V SiCMOSFET structural parameters listed below, wherein the SiC substrate thickness is 300μm and the resistivity is 0.01-0.02ohm·cm-2. The thickness of the first epitaxial layer 8 is 4μm, and the doping concentration is 8e15~1e16; the thickness of the second epitaxial layer 9 is 3μm, and the doping concentration is 3e16~1e17; the thickness of the third epitaxial layer 10 is 3μm, and the doping concentration is 1e16~1e17; taking the 1200V SiC MOSFET as an example, the total thickness of the three epitaxial layers is approximately 10μm. The primitive cell structure and process of the present invention can produce 600~10000V and above SIC MOSFET devices under a unified process platform.
[0088] like Figure 1 As shown, the structure of the first type of trench super junction MOSFET provided by the present invention, the main feature of which is a trench gate with a gate dielectric layer of uniform thickness, and another epitaxial layer below the trench gate includes a P column of a super junction structure.
[0089] Specifically, Figure 1There are three epitaxial layers on the SiC substrate 11 in sequence, including a first epitaxial layer 8, a second epitaxial layer 9 and a third epitaxial layer 10. The second epitaxial layer 9 contains the superjunction structure of the superjunction MOSFET, and the superjunction structure is composed of an N-type epitaxial layer and an N-column, and the P-column 7 of the superjunction structure is directly below the trench. The P-column 7 is formed by multiple injections of P-type ions (such as Al) at the bottom of the trench and annealing. The depth of the P-column is consistent with the thickness of the second epitaxial layer. The concentration of the P-column matches the doping concentration of the epitaxial layer that forms the superjunction structure with the P-column to achieve charge balance. The upper trench is located in the third epitaxial layer, and a gate oxide layer of uniform thickness is attached to the inside of the trench as a gate dielectric layer 5, such as a gate oxide layer, and the thickness is generally 350 to 1200Å. The polysilicon in the trench forms a trench-type gate of the MOSFET.
[0090] The surface layer of the third epitaxial layer has a P well 3, and at the same time, the two sides of the trench also have a source N+ lead-out region 1 and a P+ contact hole lead-out region 2. The surface of the epitaxial layer also has a source metal layer 4. The source metal layer 4 is connected to the source N+ lead-out region 1 and the P+ contact hole lead-out region 2 through a contact hole.
[0091] like Figure 2 FIG. 1 is a structure of a second trench super junction MOSFET provided by the present invention, which is similar to Figure 1 Compared with the structure shown in the figure, the main distinguishing feature of this structure is that the lower part of the trench has a thick field oxide layer, so that the cross-section of the gate inside the trench is torch-shaped, which is wide at the top and narrow at the bottom. Another epitaxial layer below the trench gate still contains a superjunction structure, and the P column of the superjunction structure is located directly below the trench. Between the gate at the head of the torch and the side wall of the trench is a thin gate oxide layer with a thickness of 350 to 1200Å. Between the gate at the tail handle of the torch and the side wall of the trench is a thick field oxide layer 12 with a thickness of 1000 to 3000Å. Similarly, it can also be determined whether the first epitaxial layer 8 is needed based on the actual voltage resistance requirements of the device.
[0092] The depth of the P column of the super junction structure is consistent with that of the structure 1, and the depth of the P column is consistent with the thickness of the second epitaxial layer, and at the same time meets the doping concentration requirement of the N-type region depletion.
[0093] like Figure 3 FIG. 1 is a structure of a third type of trench super junction MOSFET provided by the present invention, which is similar to Figure 1 The structure shown is Figure 2 Compared with the structure 2 shown in FIG. 1 , the main difference of the structure 3 is that the trench gate adopts a split gate structure, that is, the gate in the trench is divided into two independent gates, the upper and lower parts. Figure 2The head of the torch-shaped gate of the structure 2 shown is separated from the handle. The upper part of the groove is the device gate 6, and the lower part of the groove is the shielding electrode 13. Between the shielding electrode 13 and the sidewall of the groove, and between the device gate 6 above it, there is a thick trench field oxide layer 12. The shielding electrode 13 and the device gate 6 are both made of polysilicon, and are formed by step-by-step deposition and then back-etching. The thickness of the gate dielectric layer 5 and the trench field oxide layer 12 is consistent with the aforementioned structure 1 and structure 2. The shielding electrode 13 is connected to the source through the source metal and has the same potential as the source.
[0094] There is still a super junction structure under the trench, and the P column of the super junction structure is located directly below the trench. The depth of the P column is consistent with the thickness of the second epitaxial layer where the super junction structure is located, and its concentration also meets the doping concentration requirements for depletion of the N-type region.
[0095] The above are the primitive cell structures of three types of trench super junction MOSFETs provided by the embodiments of the present invention. The differences between them are mainly concentrated in the trench gate part, and they have different morphologies of the trench gate.
[0096] The SiC MOSFET of the present invention combines the advantages of the trench and superjunction SiC MOSFET primitive cell structures, greatly reducing the specific on-resistance per unit area (RSPA) of the SiC MOSFET. The size of the primitive cell structure is 1.0-3.0 μm, the trench depth is 2-6 μm, and the superjunction P column depth is 2-6 μm.
[0097] The trench super junction MOSFET of the above structure can be manufactured by the following embodiment process. The main difference between the three structures is concentrated in the trench gate part, and the main process steps are the same. The embodiment of the manufacturing process of the present invention adopts a three-layer epitaxial layer structure, and the first epitaxial layer 8 can be omitted in some scenarios. The specific steps are as follows: 1. First, prepare an N-type epitaxial SiC substrate wafer with three epitaxial layers. The SiC substrate thickness of the 1200V trench super junction SiC MOSFET is 300μm and the resistivity is 0.01~0.02ohm·cm-2.
[0098] The first epitaxial layer 8 has a thickness of 4 μm and a doping concentration of 8e15 to 1e16 cm-3; the second epitaxial layer 9 has a thickness of 3 μm and a doping concentration of 2e16 to 1e17 cm-3; the third epitaxial layer 10 has a thickness of 3 μm and a doping concentration of 1e16 to 1e17 cm-3. The total thickness of the three epitaxial layers of the 1200V SiC MOSFET is 10 μm.
[0099] If it is a 650V trench superjunction SiC MOSFET, the first epitaxial layer 8 is eliminated. The SiC substrate thickness is 300μm, and the doping concentration is 0.01-0.02ohm·cm-3. The second epitaxial layer 9 is 3μm thick, with a doping concentration of 2e16~1e17cm-3; the third epitaxial layer 10 is 3μm thick, with a doping concentration of 1e16~1e17cm-3. The total thickness of the two epitaxial layers of the 650V SiC MOSFET is 6μm.
[0100] That is: a set of epitaxial layer parameters selected for 1200V SiC MOSFET: The first epitaxial layer: thickness 4μm, doping concentration 1e16; The second epitaxial layer: thickness 3μm, doping concentration 1e17; The third epitaxial layer: thickness 3μm, doping concentration 4e16; A set of epitaxial layer parameters selected for 650V SiC MOSFET: The first epitaxial layer: thickness 0 μm; The second epitaxial layer: thickness 3μm, doping concentration 1e17; The third epitaxial layer: thickness 3μm, doping concentration 4e16; Then, ion implantation is performed to form a P well 3 , a source N+ lead-out region 1 , and a P+ contact hole lead-out region 2 .
[0101] Among them, the injection condition of Pwell is to adjust the injection dose according to different gate oxide thickness and threshold Vth requirements: The first implantation was Aluminum ion, with an implantation energy of 50 KeV and an implantation dose of 1.0e12 cm-2; The second implantation was Aluminum ion, with an implantation energy of 150 KeV and an implantation dose of 1.5e12 cm-2; The third implantation was Aluminum ion, with an implantation energy of 300KeV and an implantation dose of 1.5e12 cm-2.
[0102] High temperature injection conditions of source N+ lead-out region 1: First injection, Nitrogen 40Kev 4.5e14 cm-2, 500℃; Second injection, Nitrogen 70Kev 6.0e14 cm-2, 500℃; The third injection, Nitrogen 90Kev 1.0e15 cm-2, 500℃; The P+ contact hole of Pwell is led out to area 2 for injection, and an injection window is formed by photolithography and etching of a hard mask.
[0103] P+ injection conditions: The injection energy and dose are determined based on the size of the P+ injection window and the trench gate spacing. The smaller the spacing, the lower the injection energy.
[0104] The first implantation was Aluminum ion, with an implantation energy of 60 KeV, an implantation dose of 1.0e15 cm-2, and a temperature of 500 °C. The second implantation was of Aluminum ions with an implantation energy of 100 KeV, an implantation dose of 1.0e15 cm-2, and a temperature of 500°C.
[0105] 2. Trench gate and super junction structure manufacturing process. The trench process uses the traditional trench SiC MOSFET primitive cell structure formation process. After the trench is formed, high-energy P-type impurities (AL) are introduced and implanted into the second epitaxial layer at the bottom of the trench to form a super junction P column; The manufacturing process of the trench gate of structure 1 of the present invention is as follows: During trench etching, a hard mask is formed first. The hard mask is composed of a single or a combination of oxide layer / Poly / metal nickel. The thickness of the hard mask is generally 2 to 6 μm. Since the maximum injection energy of a 3 μm deep P column is about 4 MeV, the hard mask is composed of an oxide layer of 4 to 5 μm or a metal nickel of 2 to 3 μm thick. The hard mask serves as a shielding layer for trench etching and P column ion implantation.
[0106] The trench etching window of the hard mask is opened, and a trench with a depth of 2 to 6 μm is etched in the third epitaxial layer. Then, a sacrificial oxide layer with a thickness of 300 to 1000 Å is formed in the trench and wet-etched to eliminate the damage defects of the epitaxial layer caused by the trench etching.
[0107] Perform multiple super junction P column implants at the bottom of the trench: Super junction P injection, multiple high energy and high temperature injections, different epitaxial doping matches different injection doses to achieve super junction charge balance: First implantation, Aluminum ions, 20Kev 5.5e11 500℃; Second implantation, Aluminum ions, 40Kev 1.0e12 500C℃; The third implantation: Aluminum ions, 100Kev 2.0e12 500℃; The fourth implantation: Aluminum ions, 200Kev 2.2e12 500℃; The fifth implantation: Aluminum ions, 320Kev 2.8e12 500℃; The sixth implantation: Aluminum ions, 480Kev 3.4e12 500℃; The seventh implantation: Aluminum ions, 680Kev, 4.0e12, 500℃; The eighth implantation, Aluminum ions, 950Kev 4.6e12 500℃; The ninth implantation: Aluminum ions, 1250Kev, 4.6e12, 500℃; The tenth implantation: Aluminum ions, 1600Kev, 4.6e12, 500℃; The eleventh implantation: Aluminum ions, 2000Kev, 4.8e12, 500℃; The twelfth implantation, Aluminum ions, 2500Kev 4.8e12 500℃; The 13th implantation: Aluminum ions, 3000Kev, 4.8e12, 500℃; The fourteenth implantation: Aluminum ions, 3500Kev, 4.8e12, 500℃; The fifteenth implantation: Aluminum ions, 4000Kev, 4.8e12, 500℃; The sixteenth implantation: Aluminum ions, 4250Kev 2.0e12 500℃.
[0108] After the implantation is completed, thermal annealing is performed under the following conditions: 1700°C for 30 min in Ar atmosphere.
[0109] Then, a trench gate is formed in the trench. First, a 350-1200Å thick gate oxide layer 5 is formed by thermal oxidation process, and then a 12000Å thick polysilicon layer is deposited to fill the trench. Then, the polysilicon in the trench is etched back to slightly below the surface of the epitaxial layer to form a gate.
[0110] For structure 2: The manufacturing process of the trench gate of the structure 2 of the present invention is as follows: During trench etching, a hard mask is formed first. The hard mask is composed of a single or a combination of oxide layer / Poly / metal nickel. The thickness of the hard mask is generally 2 to 6 μm. Since the maximum injection energy of a 3 μm deep P column is about 4 MeV, the hard mask is composed of an oxide layer of 4 to 5 μm or a metal nickel of 2 to 3 μm thick. The hard mask serves as a shielding layer for trench etching and P column ion implantation.
[0111] The trench etching window of the hard mask is opened, and a trench with a depth of 2 to 6 μm is etched in the third epitaxial layer. Then, a sacrificial oxide layer with a thickness of 300 to 1000 Å is formed in the trench and wet-etched to eliminate the damage defects of the epitaxial layer caused by the trench etching.
[0112] Perform multiple P injections of super junction structures at the bottom of the trench: Super junction P injection, multiple high energy and high temperature injections, different epitaxial doping matches different injection doses to achieve super junction charge balance: First implantation, Aluminum ions, 20Kev 5.5e11 500℃; Second implantation, Aluminum ions, 40Kev 1.0e12 500℃; The third implantation: Aluminum ions, 100Kev 2.0e12 500℃; The fourth implantation: Aluminum ions, 200Kev 2.2e12 500℃; The fifth implantation: Aluminum ions, 320Kev 2.8e12 500℃; The sixth implantation: Aluminum ions, 480Kev 3.4e12 500℃; The seventh implantation: Aluminum ions, 680Kev, 4.0e12, 500℃; The eighth implantation, Aluminum ions, 950Kev 4.6e12 500℃; The ninth implantation: Aluminum ions, 1250Kev, 4.6e12, 500℃; The tenth implantation: Aluminum ions, 1600Kev, 4.6e12, 500℃; The eleventh implantation: Aluminum ions, 2000Kev, 4.8e12, 500℃; The twelfth implantation, Aluminum ions, 2500Kev 4.8e12 500℃; The 13th implantation: Aluminum ions, 3000Kev, 4.8e12, 500℃; The fourteenth implantation: Aluminum ions, 3500Kev, 4.8e12, 500℃; The fifteenth implantation: Aluminum ions, 4000Kev, 4.8e12, 500℃; The sixteenth implantation: Aluminum ions, 4250Kev 2.0e12 500℃.
[0113] After the implantation is completed, thermal annealing is performed under the following annealing conditions: 1700°C for 30 min in Ar atmosphere.
[0114] Then a trench gate is formed in the trench. First, a trench field oxide layer 12 with a thickness of 1000 to 3000Å is formed by oxidation, followed by the deposition of a layer of polysilicon with a thickness of 12000Å. The polysilicon is etched back to 0.6 to 1.5μm below the surface of the SiC epitaxial layer, and the trench field oxide layer is wet-etched by 0.23μm to form a thin gate oxide channel region. The polysilicon layer is then wet-etched back to remove the upper polysilicon. Thermal oxidation is performed to form a gate oxide layer 5 with a thickness of 350 to 1200Å, which is then filled with polysilicon and etched back to form a complete device gate.
[0115] For structure three: For the primitive cell structure three of the trench super junction SiC MOSFET of the present invention, the trench etching and P column implantation processes are the same as those described above. When performing the structural process inside the trench, firstly, oxidation is performed to form a trench field oxide layer 12 with a thickness of 1000 to 3000Å, and then polysilicon with a thickness of 12000Å is deposited. The polysilicon is etched back to 0.6 to 1.5μm below the surface of the SiC epitaxial layer, and the Field Oxide is wet-etched to 0.2 to 0.4μm to form a thin gate oxide channel region.
[0116] The gate oxide layer 5 is grown and the polysilicon filling and etching back of the device gate 6. The thickness of the gate oxide layer is 350-1200Å. The gate oxide layer can be generated by dry oxygen, wet oxygen or a combination of the two, and then nitrided by N2O or NO. The gate oxide layer can also be first thermally oxidized to generate a thin oxide layer, and then formed by high-temperature deposition of oxide. The polysilicon filling of the device gate 6 is to first deposit a layer of polysilicon with a thickness of 12000Å, and then etch back to 0.05-0.15μm below the surface of the SiC epitaxial layer. Unlike structure 2, this structure forms two independent gates, a lower shielding gate 13, and an upper device gate 6. The shielding electrode potential is the same as the source potential, and can be directly connected to the source electrode through a contact hole in the layout design.
[0117] Then proceed with the subsequent process. The process steps of the three structures are basically the same: The dielectric layer ILD is deposited and the source contact hole is etched.
[0118] The deposition thickness of the dielectric layer ILD is 4000-12000Å, and the dielectric layer can be composed of USG / BSG / BPSG or USG+BSG or USG+BPSG.
[0119] The contact hole is etched to form a source contact hole.
[0120] Metal Ni deposition → Ni silicide annealing and Ni removal → gate contact hole etching → metal W deposition and metal AL deposition and etching → passivation layer deposition and etching → back side thinning → back side injection → back side laser annealing → back side metal deposition.
[0121] in: The metal Ni deposition thickness is 1000Å.
[0122] Rapid thermal annealing of metal Ni: RTP800~1000℃ in nitrogen atmosphere, thermal annealing time 30~60S.
[0123] Metal Ni cleaning.
[0124] Gate contact hole etching.
[0125] Metal W deposition and metal Al deposition: Ti / TiN+W+AlSiCu sputtering process.
[0126] Metal lithography and etching.
[0127] Passivation layer deposition: SiO2 / SiN / SION+Polyimide single layer or multi-layer combination.
[0128] According to different voltage resistance specifications, the back side is thinned to a thickness of 200μm, 150μm, or 100μm.
[0129] Back side N implantation and laser annealing; Back metal deposition: Ti / Ni / Ag.
[0130] Complete chip CP test.
[0131] The cell size of the trench super junction MOSFET of the present invention is 1.0-3.0μm, the trench depth is 2-6μm deep, after the trench is etched, multiple high-energy AL injections are performed under the shielding of a hard mask to form a P-type P column structure, the concentration and width of the P column need to match the doping concentration of the second epitaxial layer in which it is located to achieve charge balance, the depth of the P column is generally 2-6μm, and during the reverse withstand voltage process of the device, the P column and N-type charges in this area are balanced, the high-concentration N-type area is depleted, and the gate oxide layer electric field in the Gate Trench area is reduced. The innovative cell structure of the present invention has different trench depths, different P column depths, and different epitaxial layer doping concentrations and thicknesses, as well as multi-layer / single-layer epitaxial layer structures / doping concentrations, all within the structural scope of the present invention.
[0132] In some embodiments, the trench region and the trench-implanted P-column superjunction structure, the total depth of the trench plus the P-column is 4 to 12 μm, the theoretical depth of the trench plus the P-column of a 600V SiC MOSFET device is 5 μm, and the theoretical depth of the trench plus the P-column of a 1200V SiC MOSFET device is 10 μm. For SiC MOSFETs with a withstand voltage exceeding 1700V, the first epitaxial layer 8 shown in the figure can be added, and the first epitaxial layer 8 with different resistivities and thicknesses can be set in combination with the original cell structure and process of the present invention. In theory, SiC MOSFETs with higher withstand voltages can be produced, such as ultra-high withstand voltage SiC MOSFETs such as 6500V and 10000V. The same set of process flows can be used to generate SiC MOSFETs with different withstand voltages, except that the first epitaxial layer uses different thicknesses and resistivities, which is one of the main advantages of the original cell structure of the present invention.
[0133] The SiC MOSFET of the present invention combines the advantages of the trench and superjunction SiC MOSFET primitive cell structures, greatly reducing the specific on-resistance per unit area (RSPA) of the SiC MOSFET.
[0134] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A primitive cell structure of a trench super junction MOSFET, characterized in that: Include: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The sidewalls in the trench have a gate dielectric layer of uniform thickness, which electrically isolates the gate conductive material filled in the trench from the epitaxial layer; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
2. The original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: The semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 ; The epitaxial layer includes at least two epitaxial layers, namely a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the groove is located in the third epitaxial layer.
3. The original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: The epitaxial layer further includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
4. The original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: In the super junction structure, the doping concentration of the P column matches the doping concentration of the epitaxial layer that forms the super junction structure with the P column, so as to achieve charge balance.
5. The original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: In the epitaxial layer, the depth of the groove is 2-6 μm, and the depth of the P column of the super junction structure is 2-6 μm.
6. The original cell structure of the trench super junction MOSFET according to claim 2, characterized in that: The thickness of the second epitaxial layer in the epitaxial layer is 3 μm, and the doping concentration is 3e16-1e17 cm -3 The thickness of the second epitaxial layer is consistent with the implantation depth of the P column; the thickness of the third epitaxial layer is 3 μm, and the doping concentration is 1e16-1e17 cm -3 .
7. The original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: The gate dielectric layer is a thin gate oxide layer with uniform thickness, and its thickness is 350-1200Å; the surface of the epitaxial layer also has a source metal layer, and the source metal layer is connected to the source N+ lead-out area and the P+ contact hole lead-out area through a contact hole.
8. A process for manufacturing the original cell structure of the trench super junction MOSFET according to claim 1, characterized in that: The process steps include: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is subsequently used to fill the gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column of a certain depth in the epitaxial layer at the bottom of the trench; Forming a gate dielectric layer on the inner wall of the trench, filling it with a gate conductive material and etching back to form the gate of the super junction MOSFET; Opening an N+ injection window by photolithography and etching, and performing N+ ion implantation to form a source N+ lead-out region of the original cell structure of the trench super junction MOSFET in the P well; Photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form a P+ contact hole lead-out area of the P well.
9. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 8, characterized in that: The semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 ; The high-energy P-type ion implantation into the epitaxial layer at the bottom of the trench to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the trench, and then multiple Al ion implantations of the P column of the super junction structure are performed; the thickness of the sacrificial oxide layer is 300 to 1000Å.
10. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 8, characterized in that: The hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or the metal nickel has a thickness of 2 to 3 μm.
11. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 9, wherein: The multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 KeV, the dose range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
12. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 11, characterized in that: The multiple Al ion implantations also include an annealing process after the implantation is completed, and the annealing conditions are 1700 degrees Celsius for 30 minutes in an argon atmosphere.
13. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 8, wherein: The ion implantation energy of the source N+ lead-out region is in the range of 40 to 90 KeV, the implantation dose is 4.5e14 to 1.0e15, and the implantation temperature is 500 degrees Celsius; the implantation conditions of the P well are adjusted according to the thickness of different gate dielectric layers and threshold requirements, and the implantation energy range is 50 to 300 KeV, and the implantation dose is 1.0e12 to 1.5e12; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, and the smaller the spacing, the lower the implantation energy; The implantation energy range is 60-100 KeV, the implantation dose is 1.0e15, and the implantation temperature is 500 degrees Celsius.
14. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 8, wherein: The process steps subsequently include depositing a metal layer on the surface of the epitaxial layer and etching to form a source metal, wherein the source metal connects the source N+ lead-out region and the P+ contact hole lead-out region.
15. A primitive cell structure of a trench super junction MOSFET, characterized in that: Include: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The trench includes the gate structure of the trench super junction MOSFET; the gate structure includes a gate and an insulating dielectric layer between the gate and the epitaxial layer; the cross section of the gate is a torch-shaped cross section morphology that is wide at the top and narrow at the bottom, a thinner gate dielectric layer is provided between the gate of the torch head at the top and the side wall of the trench, and a thicker trench field oxide layer is provided between the gate of the torch tail handle at the bottom and the side wall of the trench; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
16. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: The semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 ; The epitaxial layer includes at least two epitaxial layers, namely a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the groove is located in the third epitaxial layer.
17. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: The epitaxial layer further includes a first epitaxial layer located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage exceeding 1700V.
18. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: The doping concentration of the P column of the super junction structure matches the doping concentration of the epitaxial layer that forms the super junction structure with the P column to achieve charge balance; the depth of the P column in the super junction structure is consistent with the thickness of the second epitaxial layer, so that the P column and N-type charges are balanced when the device is reversely withstand voltage, and the high-concentration N-type area is depleted while the electric field strength of the gate dielectric layer in the trench gate area is reduced.
19. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: In the epitaxial layer, the depth of the groove is 2-6 μm, and the depth of the P column of the super junction structure, that is, the thickness of the second epitaxial layer, is 2-6 μm.
20. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: The gate has a torch-shaped head at the top and a height of 0.6 to 1.5 μm, and a thinner gate dielectric layer between the gate and the trench sidewall is 350 to 1200 Å thick; the gate has a narrower and longer torch tail handle at the bottom and a thicker trench field oxide layer between the trench sidewall is 1000 to 3000 Å thick.
21. The original cell structure of the trench super junction MOSFET according to claim 15, characterized in that: The P column is formed by combining multiple Al ion injections with different injection energies and injection doses at high temperature.
22. A process for manufacturing a primitive cell structure of a trench super junction MOSFET as claimed in claim 15, characterized in that: The process steps include: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is used for subsequent filling to form a gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column with a certain depth in the epitaxial layer at the bottom of the trench; A thicker trench field oxide layer is formed on the inner wall of the trench, a gate conductive material is filled and etched back to form a tail handle structure at the bottom of the torch-shaped gate, and then a thinner gate dielectric layer is formed on the upper part of the trench, and then the gate conductive material is continued to be filled and etched back to be flush with the surface of the epitaxial layer, so as to form a gate structure with a torch-shaped cross-section as a whole, that is, a thin gate dielectric layer is provided between the gate of the upper wider torch head and the side wall of the trench, and a thicker trench field oxide layer is provided between the gate of the lower narrow torch tail handle and the side wall of the trench; Opening an N+ injection window by photolithography and etching, and performing N+ ion implantation to form a source N+ lead-out region of the original cell structure of the trench super junction MOSFET in the P well; Photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form a P+ contact hole lead-out area of the P well.
23. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 22, wherein: The epitaxial layer at least includes a second epitaxial layer and a third epitaxial layer; the second epitaxial layer contains the super junction structure of the super junction MOSFET, and the third epitaxial layer contains the gate structure of the super junction MOSFET.
24. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 23, characterized in that: The epitaxial layer further comprises a first epitaxial layer, which is located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage of more than 1700V; the thickness of the first epitaxial layer is 4μm, and the doping concentration is 8e15-1e16cm -3 .
25. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 23, characterized in that: The thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm -3 The thickness of the third epitaxial layer is 3 μm, and the doping concentration is 1e16-1e17 cm -3 .
26. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 22, wherein: The high-energy P-type ion implantation into the epitaxial layer at the bottom of the trench to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the trench, and then multiple Al ion implantations of the P column of the super junction structure are performed; the thickness of the sacrificial oxide layer is 300 to 1000Å; The multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 Kev, the dosage range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
27. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 22, wherein: The hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or the metal nickel has a thickness of 2 to 3 μm.
28. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 26, wherein: The multiple Al ion implantations also include an annealing process after the implantation is completed. The annealing conditions are 1700° C. for 30 minutes in an argon atmosphere.
29. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 22, wherein: A thicker trench field oxide layer is formed on the inner wall of the trench, the thickness of the trench field oxide layer is 1000-3000Å, and after depositing the gate conductive material, it is etched back, the etching depth is 0.6-1.5μm from the top surface of the epitaxial layer downward, and the 0.1-0.3μm thickness of the trench field oxide layer is removed by wet etching to form a channel region, and then the upper gate conductive material is etched away; then a gate dielectric layer with a thickness of 350-1200Å is formed on the inner wall of the upper part of the trench, polysilicon is deposited and etched back to form a gate with a complete structure.
30. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 22, wherein: The ion implantation energy range of the source N+ lead-out region is 40-90KeV, the implantation dose is 4.5e14-1.0e15, and the implantation temperature is 500°C; the implantation conditions of the P well are adjusted according to the thickness and threshold requirements of different gate dielectric layers, and the implantation energy range is 50-300KeV, and the implantation dose is 1.0e12-1.5e12; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, and the smaller the spacing, the lower the implantation energy; The implantation energy range is 60-100 KeV, the implantation dose is 1.0e15, and the implantation temperature is 500°C.
31. A primitive cell structure of a trench super junction MOSFET, characterized in that: Include: Providing a semiconductor substrate, wherein the semiconductor substrate comprises an epitaxial layer; The epitaxial layer includes a primitive cell structure of the trench super junction MOSFET, wherein the trench constitutes a gate of the super junction MOSFET, and a super junction structure is provided below the trench; The super junction structure comprises a P column and an N column; the P column is located directly below the groove and is in contact with the bottom surface of the groove; the N column is composed of the epitaxial layer; The trench contains the gate structure of the trench super junction MOSFET; the gate structure is a separated gate structure consisting of two independent parts, upper and lower; wherein the shielding gate located at the lower part of the trench is in the shape of an elongated rod, and a thicker trench field oxide layer is provided between the shielding gate and the trench sidewall; the lateral width of the device gate located at the upper part of the trench is greater than that of the shielding gate, and the longitudinal length of the device gate is less than that of the shielding gate; and a gate dielectric layer thinner than the thickness of the trench field oxide layer is provided between the device gate and the trench sidewall; The epitaxial layer near the upper part of the trench has a P well of the trench super junction MOSFET, and the surface epitaxial layer of the P well includes a source N+ lead-out region of the trench super junction MOSFET and a P+ contact hole lead-out region of the P well that is in contact with the source N+ lead-out region.
32. The original cell structure of the trench super junction MOSFET according to claim 31, characterized in that: The semiconductor substrate is a silicon carbide substrate with a thickness of 300 μm and a resistivity of 0.01 to 0.02 ohm·cm. -2 The epitaxial layer comprises at least two epitaxial layers, namely, a second epitaxial layer and a third epitaxial layer; the super junction structure is formed in the second epitaxial layer, the third epitaxial layer is located on the second epitaxial layer, and the groove is located in the third epitaxial layer; the thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm -3 The thickness of the third epitaxial layer is 3 μm, and the doping concentration is 1e16-1e17 cm -3 .
33. The original cell structure of the trench super junction MOSFET according to claim 32, characterized in that: The epitaxial layer further comprises a first epitaxial layer, which is located between the second epitaxial layer and the semiconductor substrate, so as to achieve a higher withstand voltage exceeding 1700V; The thickness of the first epitaxial layer is 4 μm, and the doping concentration is 8e15-1e16 cm -3 .
34. The original cell structure of the trench super junction MOSFET according to claim 31, characterized in that: The depth of the groove is 2 to 6 μm, and the thickness of the second epitaxial layer is consistent with the depth of the P column of the super junction structure, so that the high-concentration epitaxial layer N-type region is depleted while the electric field strength of the gate dielectric layer of the groove is reduced; the longitudinal length of the device gate at the top of the groove is 0.6 to 1.5 μm, and the thickness of the gate dielectric layer is 350 to 1200 Å; the thickness of the trench field oxide layer around the shielding gate is 1000 to 3000 Å.
35. The original cell structure of the trench super junction MOSFET according to claim 31, characterized in that: The P column is formed by combining multiple Al ion injections with different injection energies and injection doses at high temperature.
36. A process for manufacturing a primitive cell structure of a trench super junction MOSFET as claimed in claim 31, characterized in that: The process steps include: Providing a semiconductor substrate, and forming an epitaxial layer on the semiconductor substrate; P-type ion implantation forms a P-well; Forming a hard mask layer, performing a trench etching process, defining a trench area through the hard mask, etching the epitaxial layer to form a trench, and the trench is used for subsequent filling to form a gate of the trench super junction MOSFET; After the trench etching is completed, high-energy P-type ions are implanted into the epitaxial layer at the bottom of the trench to form a P column with a certain depth in the epitaxial layer at the bottom of the trench; A thicker trench field oxide layer is formed on the inner wall of the trench, and then a gate conductive material is deposited and back-etched to form a shielding gate at the bottom; then the trench field oxide layer is wet-etched to a certain thickness to form a channel region; then a thin gate dielectric layer is formed, and a gate conductive material is deposited and back-etched to form a device gate; the shielding gate and the device gate are electrically isolated from each other by the trench field oxide layer; Opening an N+ injection window by photolithography and etching, and performing N+ ion implantation to form a source N+ lead-out region of the original cell structure of the trench super junction MOSFET in the P well; Photolithography and etching are performed again to open the P+ injection window, and P+ ion implantation is performed to form a P+ contact hole lead-out area of the P well.
37. The process for producing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The epitaxial layer at least comprises a second epitaxial layer and a third epitaxial layer; the second epitaxial layer comprises a super junction structure of the super junction MOSFET, the third epitaxial layer comprises a groove, and the groove comprises a gate structure of a separate gate structure of the super junction MOSFET; the thickness of the second epitaxial layer is 3um, and the doping concentration is 2e16-1e17cm -3 The thickness of the third epitaxial layer is 3 μm, and the doping concentration is 1e16-1e17 cm -3 .
38. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The epitaxial layer further comprises a first epitaxial layer, which is located between the second epitaxial layer and the semiconductor substrate to achieve a higher withstand voltage of more than 1700V; the thickness of the first epitaxial layer is 4μm, and the doping concentration is 8e15-1e16cm -3 .
39. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The width of the trench and the thickness of the trench field oxide layer or gate dielectric layer on both sides of the trench need to match the thickness and concentration of the third epitaxial layer; the thickness of the third epitaxial layer is consistent with the depth of the trench, and the thickness of the second epitaxial layer is consistent with the depth of the P column formed by multiple high-energy implantations; While depleting the high-concentration N-type region, the electric field of the gate dielectric layer in the trench gate region is reduced.
40. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The high-energy P-type ion implantation into the epitaxial layer at the bottom of the groove to form the P column of the super junction structure is formed by multiple Al ion implantations; before the multiple Al ion implantations, a sacrificial oxide layer is first formed inside the groove, and then multiple Al ion implantations are performed to form the P column of the super junction structure; the thickness of the sacrificial oxide layer is 300 to 1000Å.
41. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The hard mask layer is any single material layer of oxide layer, polysilicon, and metal nickel, or any combination thereof; when it is a single material layer, the oxide layer has a thickness of 4 to 5 μm, or the metal nickel has a thickness of 2 to 3 μm.
42. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 40, wherein: The multiple Al ion implantations of the P column have an implantation depth of 2 to 6 μm, which is consistent with the thickness of the second epitaxial layer; the energy range of the multiple Al ion implantations is 20 to 4250 KeV, the dose range is 5.5e11 to 4.8e12, and the implantation temperature is 500°C.
43. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 40, wherein: After the multiple Al ion implantations to form the P columns, an annealing process is also included, and the annealing conditions are 1700° C. / 30 min in an argon atmosphere.
44. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: A thicker trench field oxide layer is formed on the inner wall of the trench, the thickness of the trench field oxide layer is 1000-3000Å, and after depositing the gate conductive material, it is etched back, the etching depth is 0.6-1.5μm from the top surface of the epitaxial layer downward, forming a lower shielding electrode; the trench field oxide layer is wet-etched to a thickness of 0.2-0.4μm to form a channel region; and then a gate dielectric layer with a thickness of 350-1200Å is formed on the upper inner wall of the trench, polysilicon is deposited and etched back to form the upper device gate.
45. The process for manufacturing a primitive cell structure of a trench super junction MOSFET according to claim 36, wherein: The ion implantation energy of the source N+ lead-out region is in the range of 40 to 90 KeV, the implantation dose is 4.5e14 to 1.0e15, and the implantation temperature is 500 degrees Celsius; the implantation conditions of the P well are adjusted according to the thickness of different gate dielectric layers and threshold requirements, and the implantation energy range is 50 to 300 KeV, and the implantation dose is 1.0e12 to 1.5e12; the implantation window of the P+ contact hole lead-out region determines the implantation energy and dose according to the spacing between the P+ implantation window and the trench gate, and the smaller the spacing, the lower the implantation energy; The implantation energy range is 60-100 KeV, the implantation dose is 1.0e15, and the implantation temperature is 500°C.