Ni-Fe-Mn-based layered oxide sodium ion positive electrode material as well as preparation method and application thereof

By combining the sol-gel method and wet chemical method, Ni-Fe-Mn layered oxide sodium-ion cathode material was prepared, which solved the problems of short cycle life and air sensitivity of sodium-ion battery cathode materials, and achieved high first-cycle discharge specific capacity and good cycle stability.

CN118969977APending Publication Date: 2024-11-15QINGDAO FUSION EQUIP TECH CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410871650.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials suffer from problems such as short cycle life, high air sensitivity, and unstable electrochemical performance, and single modification methods are insufficient to effectively improve their performance.

Method used

A combination of sol-gel and wet chemical methods was used to form Ni-Fe-Mn basal oxide sodium ion cathode material through metal element doping and oxide surface modification. The specific steps included mixed solution preparation, gel formation, drying, heat treatment and surface coating to form a dense oxide film to improve the material stability.

Benefits of technology

It achieves high first-cycle discharge specific capacity and good cycle stability, with a first-cycle discharge specific capacity of over 100 mAh/g, high cycle retention, and significantly improved material structural stability and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969977A_ABST
    Figure CN118969977A_ABST
Patent Text Reader

Abstract

The invention discloses a Ni-Fe-Mn-based layered oxide sodium ion positive electrode material as well as a preparation method and application thereof, and belongs to the technical field of battery positive electrode materials. According to the technical scheme, the general formula is NamNixFeyM11-x-y-nMnnO2, and the preparation method comprises the following steps: 1) preparing a sodium source, a nickel source, a manganese source, an iron source and an M1 metal source into a mixed solution, and stirring; 2) adding a chelating agent; 3) heating and stirring the mixed solution to evaporate water until gel is formed, and drying; 4) grinding the dried gel, and collecting the ground gel into a corundum crucible for subsequent heat treatment; and 5) a heat treatment process: sintering twice to obtain the target positive electrode material. The sodium ion battery positive electrode material is easy in chemical reaction, short in preparation period, low in cost and capable of being combined with metal ions to form a stable complex, and the positive electrode material prepared by a sol-gel method can realize uniform mixing or doping at a molecular level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery positive electrode materials, and specifically relates to a Ni-Fe-Mn based layered oxide sodium ion positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries (LIBs) have been widely used in electric vehicles, portable electronic devices, energy storage systems, aerospace, etc., and have been recognized by the world for their high energy density, portability and environmental friendliness. However, the limited reserves of lithium resources have hindered its continued application. Sodium-ion batteries have good application prospects because of their lower manufacturing costs than lithium batteries. Layered transition metal oxides, as a type of positive electrode material for sodium-ion batteries, have attracted widespread attention due to their simple structure, easy synthesis and high specific capacity. It is a layered structure formed by alternating transition metal layers (Fe, Co, Ni, Cu, Zn, etc.) and alkali metal layers, and the general formula is NaTMO 2 (TM is transition metal). According to Na + The coordination configuration and O 2- The stacking method of layered transition metal oxides is divided into four different structures: O3, O2, P3 and P2. Among them, layered transition metal oxides with O3 and P2 phase structures are the main positive electrode materials for sodium ion batteries. However, problems such as short cycle life and high air sensitivity limit their commercial development.

[0003] The electrochemically active elements of cationic redox are mainly Sc, Ti, Fe, Co, Ni, Cu and lanthanide metals (Ce, Dy, Nd, etc.). These elements have their own unique redox characteristics and their voltage ranges for charge compensation are also different. 2+ Occurrence of Ni 2+ / Ni 3+ and Ni 3+ / Ni 4+ The redox reaction has an average redox voltage of more than 3V; Mn 2+ Redox reaction occurs in the low pressure region to generate Mn 3+ , while high spin Mn 3+ The Jahn-Teller effect can cause serious distortion and disproportionation reactions in the sodium cathode material, thereby destroying the stability of the layered structure; Fe is cheap, and if the Fe content is relatively high, Fe 3+ migration, anion redox, and Fe 4+The triggered surface side reactions lead to capacity decay of the sodium cathode material, thus reducing the cycle life of the material. Different combinations of transition metal layer components in different systems will result in different structural characteristics of the material and different effects on the electrochemical performance. Even the same element may have different charge compensation mechanisms in different materials. Different modification choices for the same modification method will lead to large differences in material performance.

[0004] P2 type Na 2 / 3 Ni 1 / 3 Mn 2 / 3 O 2 (NNMO) layered oxides have been widely studied due to their low manufacturing cost and adaptability to a wide temperature range, but their cycle stability and rate performance are poor. Therefore, Liu et al. greatly improved the P2-type Na by adjusting the proportion of Na (Nae / Naf ratio). 2 / 3 Ni 1 / 3 Mn 2 / 3 O 2 (NNMO) cycle life (Adv.Energy Mater.2023,13,2203521) and rate performance, Na 0.696 Ni 0.329 Mn 0.671 O 2 The capacity retention rate of (NM-2) after 1000 cycles at 1C is 71.9%, and the specific capacity at 50C is 54.33 mAh g -1 Sun Xueliang et al. studied the coating material (Al 2 O 3 、ZrO 2 and TiO 2 ) for P2-Na 0.66 (Mn 0.54 Co 0.13 Ni 0.13 ) 2 The impact of Al 2 O 3 Can improve material stability, ZrO 2 The rate performance of the material can be improved, and TiO 2 It can easily promote the decomposition of the electrolyte and the occurrence of side reactions, thus destroying the electrochemical properties of the material itself.

[0005] In view of the above reports and the problems existing in the current sodium cathode materials, in order to improve their cycle life and stability in air, surface coating (TiO 2 Coating, Al 2 O 3 Coating and CaTiO 3 coating, etc.), transition metal doping (Li + , Cu2+ , Ti 4+ , Mg 2+ and Al 3+ etc.), morphology regulation (core-shell composite structure, nanosheets, etc.), and other modification methods to improve the cycle life and air stability of the material. However, using only a single modification method still cannot effectively improve the capacity and voltage stability, making it difficult to achieve practical applications. Summary of the Invention

[0006] The present invention provides a Ni-Fe-Mn-based layered oxide sodium-ion cathode material, its preparation method and application. The sodium-ion cathode material of the present invention is a modified material formed by combining metal element doping and oxide surface modification through two strategies of sol-gel method and wet chemical method, which can take into account the advantages of both doping and surface modification.

[0007] The technical solution of the present invention is as follows:

[0008] In the first aspect, a Ni-Fe-Mn-based layered oxide sodium-ion cathode material is disclosed, with the general formula Na m Ni x Fe y M1 1-x-y-n Mn n O 2 , where 0 < m ≤ 1, 0 < x < 0.5, 0 < y < 0.5, 0 < n < 1, and M1 is one or more of Li, Cu, Mg, Ti, Al, or Zn.

[0009] In the second aspect, a preparation method of the Ni-Fe-Mn-based layered oxide sodium-ion cathode material is disclosed, including the following steps:

[0010] 1) Prepare a mixed solution of a sodium source, a nickel source, a manganese source, an iron source, or a sodium source, a nickel source, a manganese source, an iron source, and an M1 metal source, and stir for 1 - 8 h;

[0011] 2) Add a chelating agent and stir for 2 - 6 h to form a transparent mixed solution;

[0012] 3) Transfer the mixed solution to an oil bath at 70 - 95 °C and heat for 3 - 5 h, continuously stirring to evaporate water until a gel is formed, and then transfer the gel to a forced-air drying oven and dry for 6 - 12 h;

[0013] 4) Grind the dried gel, and then collect it in a corundum crucible for subsequent heat treatment;

[0014] 5) Heat treatment process: First, sinter at 400 - 600 °C for 4 - 8 h, and then sinter at 800 - 950 °C for 10 - 20 h, with a heating rate of 1 - 5 °C·min -1 , and Na m Nix Fe y M1 1-x-y-n Mn n O 2 Positive electrode material.

[0015] Preferably, in step 1), the sodium source is one of sodium nitrate, sodium chloride, sodium sulfate, sodium carbonate or sodium acetate; more preferably, the sodium source is one of sodium nitrate, sodium acetate, sodium sulfate and sodium chloride.

[0016] Preferably, the nickel source in step 1) is any one of nickel nitrate, nickel acetate, nickel sulfate or nickel chloride, or a combination mixture of at least two of them; more preferably, the nickel source is one of nickel nitrate, nickel acetate, nickel sulfate or nickel chloride.

[0017] Preferably, in step 1), the manganese source is any one of manganese nitrate, manganese acetate, manganese sulfate or manganese chloride, or a combination mixture of at least two of them; the manganese source is one of manganese nitrate, manganese acetate, manganese sulfate or manganese chloride.

[0018] Preferably, in step 1), the iron source is any one of iron nitrate, iron sulfate or iron chloride, or a combination mixture of at least two of them; the iron source is one of ferric nitrate, ferrous sulfate or ferric chloride.

[0019] Preferably, in step 1), the M1 metal source is a mixture of one or more of nitrates, acetates, sulfates or chlorides of Li, Cu, Mg, Ti, Al or Zn.

[0020] Preferably, in step 2), the chelating agent is citric acid and oxalic acid, and the ratio of the sum of the amounts of the sodium source, nickel source, manganese source, iron source or the sodium source, nickel source, manganese source, iron source and M1 metal source to the amount of the chelating agent is 1:(1.0-1.1).

[0021] In the third aspect, a surface-modified sodium ion positive electrode material is disclosed, which is prepared using the Ni-Fe-Mn based oxide sodium ion positive electrode material, specifically: dissolving the metal source M2 in anhydrous ethanol and continuously stirring to form a solution, and then m Ni x Fe y M1 1-x-y-n Mn n O 2 The positive electrode material is dispersed in anhydrous ethanol and stirred to form a solution. The ethanol solution containing the metal source M2 and the ethanol solution containing Na m Ni x Fe y M1 1-x-y-n Mn n O 2The ethanol solution of the positive electrode material is mixed and continuously stirred and heated in a 50-90°C oil bath until the ethanol is completely volatilized, and then the obtained mixture is ground and calcined in a 400-900°C muffle furnace for 6-15h to finally obtain the surface-modified sodium ion positive electrode material NNFMM-Al-Zn sodium ion battery positive electrode material.

[0022] In a fourth aspect, the application of the Ni-Fe-Mn based layered oxide sodium ion positive electrode material in a sodium ion battery is disclosed.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The chemical reaction for preparing the positive electrode material of the sodium ion battery provided by the present invention is easy to carry out, the preparation cycle is short, the cost is low, and the addition of a chelating agent can combine with metal ions to form a stable complex, and the positive electrode material prepared by the sol-gel method can achieve uniform mixing or doping at the molecular level;

[0025] 2. The NNFMM-Al-Zn sodium ion battery positive electrode material provided by the present invention has a first-cycle discharge capacity of more than 100 mAh / g. At a current density of 1C, the first-cycle discharge capacity is 117.1 mAh / g, and the cycle retention rate is 100%;

[0026] 3. The present invention uses a variety of metal elements for surface coating, which can form a dense oxide film on its surface and increase the stability of the positive electrode material in the air;

[0027] 4. Doping with a small amount of Mg 2+ It can effectively inhibit harmful phase changes of layered materials under high voltage, reduce their volume strain, improve the structural stability of materials, and increase the redox reaction activity of active elements in materials, thereby increasing the energy density of materials;

[0028] 5.Al 2 O 3 and ZnO are coated on the surface of the material. On the one hand, as a protective layer, they can isolate the electrode material from direct contact with the electrolyte and surface side reactions, and hinder the embedding of solvent molecules and anions in the electrolyte into the layered material under high voltage; on the other hand, Al and Zn have good electronic conductivity and good compatibility with Mg-doped layered materials, which can effectively improve their rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is the XRD diagram of the positive electrode material prepared in Examples 1-3 of the present invention.

[0030] Figure 2 This is a cycle stability curve of a battery prepared using the positive electrode material of Example 1 as an active material at a current density of 0.1C.

[0031] Figure 3 This is a cycle stability curve of a battery prepared using the positive electrode material of Example 1 as an active material at a current density of 1C.

[0032] Figure 4 This is a cycle stability curve of a battery prepared using the positive electrode material of Example 1 as an active material at a current density of 5C.

[0033] Figure 5 This is a cycle stability curve of a battery prepared using the positive electrode material of Example 2 as an active material at a current density of 1C.

[0034] Figure 6 Cyclic stability curve of a battery prepared using the cathode material of Example 3 as an active material at a current density of 1C.

[0035] Figure 7 The first cycle charge and discharge curve of the battery prepared by the present invention using the positive electrode material of Comparative Example 1 as the active material at a current density of 1C.

[0036] Figure 8 The first cycle charge and discharge curve of the battery prepared by the present invention using the positive electrode material of Comparative Example 2 as the active material at a current density of 1C.

[0037] Fig. 9 The first cycle charge and discharge curve of the battery prepared by using the positive electrode material of Comparative Example 3 as the active material at a current density of 1C.

[0038] Fig.10 The first cycle charge and discharge curve of the battery prepared by using the positive electrode material of Comparative Example 4 as the active material at a current density of 1C.

[0039] Fig.11 The first cycle charge and discharge curve of the battery prepared by using the positive electrode material of Comparative Example 5 as the active material at a current density of 1C. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0041] Example 1

[0042] The preparation method of the Ni-Fe-Mn based layered oxide sodium ion positive electrode material is specifically as follows:

[0043] 1) 4.98 g nickel acetate, 10.11 g ferric nitrate, 13.48 g manganese acetate and 6.72 g sodium acetate (5 mol% excess) were prepared into a mixed solution with a concentration of 0.1 mol / L, and stirred on a magnetic stirrer for 3 h;

[0044] 2) On the basis of step 1), 19.4 g of citric acid and 8.9 g of oxalic acid were added and stirred for 3 h to form a transparent green mixed solution;

[0045] 3) The mixed solution was transferred to an 85°C oil bath and heated for 4 h, with continuous stirring until the water was completely evaporated to form a gel, and then the gel was transferred to an air drying oven and dried for 6 h;

[0046] 4) grinding the dried xerogel and collecting it into a corundum crucible for subsequent heat treatment;

[0047] 5) Heat treatment process: first sinter at 520℃ for 6 hours, then sinter at 950℃ for 15 hours, with a heating rate of 3℃·min -1 After the program is finished, you can get Na 0.78 Ni 0.2 Fe 0.25 Mn 0.55 O 2 Positive electrode material.

[0048] Example 2

[0049] The preparation method of the Ni-Fe-Mn based layered oxide sodium ion positive electrode material is specifically as follows:

[0050] 1) 2.49 g nickel acetate, 10.11 g ferric nitrate, 13.48 g manganese acetate, 2.14 g magnesium acetate and 6.72 g sodium acetate (5 mol% excess) were prepared into a mixed solution with a concentration of 0.1 mol / L, and stirred on a magnetic stirrer for 3 h;

[0051] 2) On the basis of step 1), 19.4 g of citric acid and 8.9 g of oxalic acid were added and stirred for 3 h to form a transparent green mixed solution;

[0052] 3) The mixed solution was transferred to an 85°C oil bath and heated for 4 h, with continuous stirring until the water was completely evaporated to form a gel, and then the gel was transferred to an air drying oven and dried for 6 h;

[0053] 4) grinding the dried xerogel and collecting it into a corundum crucible for subsequent heat treatment;

[0054] 5) Heat treatment process: first sinter at 520℃ for 6 hours, then sinter at 950℃ for 15 hours, with a heating rate of 3℃·min -1After the program is finished, you can get Na 0.78 Ni 0.1 Fe 0.25 Mn 0.55 Mg 0.1 O 2 Positive electrode material.

[0055] Example 3

[0056] The preparation method of the surface-modified sodium ion positive electrode material NNFMM-Al-Zn is specifically as follows:

[0057] In Example 2, Na 0.78 Ni 0.1 Fe 0.15 Mn 0.65 Mg 0.1 O 2 Based on the positive electrode material, the surface is modified;

[0058] a) Dissolve 1.0 g aluminum nitrate and 0.5 g zinc nitrate in 40 mL anhydrous ethanol and continue stirring to dissolve;

[0059] b) Na prepared in Example 2 0.78 Ni 0.1 Fe 0.25 Mn 0.55 Mg 0.1 O 2 The cathode material was dissolved and dispersed in 40 mL of anhydrous ethanol and stirred continuously to form a uniform solution;

[0060] c) The solutions of step a) and step b) are mixed, and heated in an oil bath at 70° C. with continuous stirring until the ethanol is completely evaporated.

[0061] d) grinding the mixture of step c) and calcining in a muffle furnace at 750° C. for 15 h to finally obtain a surface-modified sodium ion positive electrode material NNFMM-Al-Zn.

[0062] The sodium positive electrode materials obtained in Examples 1-3 were subjected to XRD testing. Figure 1 As shown, the XRD of Example 1 shows a pure phase structure with good crystallinity. Examples 2 and 3 also show diffraction peaks similar to those of Example 1, which indicates that a small amount of Mg 2+ Doping and Al 2 O 3 , ZnO surface modification will not affect the crystal structure of the material.

[0063] Comparative Example 1

[0064] The difference from Example 1 is that the amount of sodium acetate added in this comparative example is 6.4 g (the addition of sodium acetate is not excessive), and the other steps and methods are the same as those in Example 1.

[0065] Comparative Example 2

[0066] The difference from Example 2 is that this comparative example does not include step 2) the addition of a chelating agent, and the other steps and methods are the same as those of Example 1.

[0067] Comparative Example 3

[0068] The difference from Example 3 is that in step a), only 5 wt% aluminum nitrate based on the total mass of the positive electrode material is added, and zinc nitrate is not added. The other steps and methods are different from those in Example 3.

[0069] Comparative Example 4

[0070] Different from Example 2, in step 5) of this comparative example, the heating rate is 10°C·min -1 .

[0071] Comparative Example 5

[0072] Different from Example 2, in step 2) of this comparative example, the amount of citric acid added is 38.2 g.

[0073] The positive electrode materials prepared in Examples 1-3 and Comparative Examples 1-5 were used as positive electrode active materials, and aluminum foil was used as positive electrode current collector. The positive electrode sheet was prepared by conventional methods in the art: the positive electrode sheet was prepared by dispersing the positive electrode active material, conductive carbon black (Super P) and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) at a ratio of 7:2:1 to obtain a positive electrode slurry, which was coated on aluminum foil, dried, and pressed; sodium sheet was used as counter electrode and reference electrode, and the electrolyte was 1M NaClO 4 The cathode material of Example 1 was dissolved in PC (polycarbonate), and 5% FEC (fluoroethylene carbonate) was added as an additive. The separator was a glass fiber separator (Whatman, GF / F). The battery was assembled using a CR2016 button battery, and the battery cycle stability performance test was performed. The cycle stability curve of the battery prepared using the cathode material of Example 1 as the active material at a current density of 0.1C was as shown in FIG. Figure 2 The cycling stability curve at 1C current density is shown in Figure 3 As shown in the figure, the cycling stability curve at 5C current density is Figure 4 As shown; the cycle stability curve of the battery prepared using the positive electrode material of Example 2 as the active material at 1C current density is as shown Figure 5 As shown; the cycle stability curve of the battery prepared using the positive electrode material of Example 3 as the active material at 1C current density is as shown Figure 6 As shown. Figure 2-6 It can be seen that at a low rate of 0.1C, after 10 cycles, the battery prepared using the positive electrode material of Example 1 as the active material has a discharge capacity of 101.1mAh / g, and the capacity retention rate is as high as 100%. At 1C, the first cycle discharge capacity is 97.2mAh / g, and the cycle retention rate is 100%. At 5C, the first cycle discharge capacity is 79.0mAh / g, and the cycle retention rate is 99.8%; the battery prepared using the positive electrode material of Example 2 as the active material has a first cycle discharge capacity of 103.6mAh / g at a current density of 1C, and a cycle retention rate of 100%; the battery prepared using the positive electrode material of Example 3 as the active material has a first cycle discharge capacity of 117.1mAh / g at a current density of 1C, and a cycle retention rate of 100%. It can be seen that at a current density of 1C, the modified sodium ion positive electrode material NNFMM-Al-Zn has a more significant difference in cycle stability, showing a more significantly improved electrochemical performance.

[0074] like Figure 7 As shown, the battery prepared with the positive electrode material of Comparative Example 1 as the active material has a first-cycle discharge capacity of 92.1 mAh / g at a current density of 1C, which is significantly lower than that of Example 1, because insufficient sodium ion content will affect the grain size and crystallinity of the material, thereby leading to a decrease in electrochemical performance, such as a decrease in discharge capacity and poor cycle stability.

[0075] like Figure 8 As shown, the battery prepared with the positive electrode material of Comparative Example 2 as the active material has a first-cycle discharge specific capacity of 89.4 mAh / g at a current density of 1C. Failure to add citric acid and oxalic acid as chelating agents may lead to uneven distribution of the positive electrode material components and a larger particle size. The larger particle size and uneven composition lead to a decrease in the ion migration rate and poor cycle stability, resulting in a decrease in the electrochemical performance of the positive electrode material.

[0076] like Fig. 9 As shown, the battery prepared with the positive electrode material of Comparative Example 3 as the active material has a first cycle discharge capacity of 108.2 mAh / g at a current density of 1C, but is inferior to that of Example 3. 2 O 3 ) as a coating layer of the positive electrode material can significantly improve the electrochemical performance of the battery. Zinc oxide (ZnO) as another coating material also has the effect of improving battery performance. When highly conductive aluminum-doped zinc oxide is used as a coating layer, it can reduce the contact between the positive electrode material and the electrolyte, inhibit the occurrence of side reactions, and improve the problem of poor conductivity of the material itself, enhance the rate performance, and aluminum oxide and zinc oxide work together to improve the battery performance in Example 3.

[0077] like Fig.10 As shown, the battery prepared with the positive electrode material of Comparative Example 2 as the active material has a first-cycle discharge specific capacity of 97 mAh / g at a current density of 1C, which is significantly lower than that of Example 2. The heating rate will affect the physical and chemical properties and structural characteristics of the positive electrode material of the sodium ion battery. A slower heating rate may contribute to the orderly arrangement and stable occupation of sodium ions in the layered structure, thereby improving the electrochemical properties of the material. Within a certain range, the heating rate will not affect the crystallinity of the material. A faster heating rate may have an adverse effect on the degree of crystallization, characteristic diffraction peak intensity, and stability of the positive electrode material of the sodium ion battery, causing the electrochemical performance of the material to decline.

[0078] like Fig.11 As shown, the battery prepared with the positive electrode material of Comparative Example 2 as the active material has a first-cycle discharge capacity of 102.6 mAh / g at a current density of 1C. Only citric acid is added as a chelating agent, and its electrochemical performance is slightly lower than that of Example 2. Oxalic acid can stabilize sodium ions and reduce their transmission resistance in the electrolyte; citric acid can inhibit material agglomeration, making the positive electrode material regular in morphology and uniform in particle size distribution. The synergistic effect of the two can effectively stabilize the crystal structure of the material, facilitate the rapid migration of sodium ions, and improve the reversibility of electrochemistry.

Claims

1. Ni-Fe-Mn based oxide sodium ion positive electrode material, characterized in that: The general formula is Na m Ni x Fe y M1 1-x-y- n Mn n O2, where 0 < m ≤ 1, 0 < x < 0.5, 0 < y < 0.5, 0 < n < 1, and M1 is one or more of Li, Cu, Mg, Ti, Al, or Zn.

2. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 1, characterized in that: The following steps are involved: 1) Prepare a mixed solution of sodium source, nickel source, manganese source, iron source or sodium source, nickel source, manganese source, iron source and M1 metal source, and stir for 1-8h; 2) adding a chelating agent and stirring for 2-6 hours to form a transparent mixed solution; 3) Transfer the mixed solution to a 70-95°C oil bath and heat for 3-5 hours, stirring continuously to evaporate the water until a gel is formed, and then transfer the gel to a forced air drying oven and dry for 6-12 hours; 4) grinding the dried gel and collecting it into a corundum crucible for subsequent heat treatment; 5) Heat treatment process: first sinter at 400-600℃ for 4-8h, then sinter at 800-950℃ for 10-20h, with a heating rate of 1-5℃·min -1 , you can get Na m Ni x Fe y M1 1-x-y-n Mn n O2 positive electrode material.

3. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In the step 1), the sodium source is one of sodium nitrate, sodium chloride, sodium sulfate, sodium carbonate or sodium acetate.

4. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In the step 1), the nickel source is any one of nickel nitrate, nickel acetate, nickel sulfate or nickel chloride, or a combination of at least two of them.

5. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In the step 1), the manganese source is any one of manganese nitrate, manganese acetate, manganese sulfate or manganese chloride, or a combination of at least two of them.

6. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In step 1), the iron source is any one of iron nitrate, iron sulfate or iron chloride, or a combination of at least two of them.

7. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In the step 1), the M1 metal source is one or more combinations of nitrates, acetates, sulfates or chlorides of Li, Cu, Mg, Ti, Al or Zn.

8. The method for preparing the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 2, characterized in that: In step 2), the chelating agent is citric acid and oxalic acid, and the ratio of the sum of the amounts of the sodium source, nickel source, manganese source, iron source or the sodium source, nickel source, manganese source, iron source and M1 metal source to the amount of the chelating agent is 1:(1.0-1.1).

9. A surface-modified sodium ion positive electrode material, characterized in that: The method is prepared by using the Ni-Fe-Mn based oxide sodium ion positive electrode material as claimed in claim 1, specifically: dissolving the metal source M2 in anhydrous ethanol and continuously stirring to form a solution, and then m Ni x Fe y M1 1-x-y-n Mn n The O2 positive electrode material is dispersed in anhydrous ethanol and stirred to form a solution. The ethanol solution containing the metal source M2 and the ethanol solution containing Na m Ni x Fe y M1 1-x-y-n Mn n The ethanol solution of the O2 positive electrode material is mixed and continuously stirred and heated in a 50-90°C oil bath until the ethanol is completely volatilized, and then the obtained mixture is ground and calcined in a 400-900°C muffle furnace for 6-15h to finally obtain the surface-modified sodium ion positive electrode material NNFMM-Al-Zn sodium ion battery positive electrode material.

10. Use of the Ni-Fe-Mn based layered oxide sodium ion positive electrode material according to claim 1 in a sodium ion battery.

Citation Information

Cited By

  • Layered positive electrode material of high-capacity sodium-ion battery as well as preparation method and application of layered positive electrode material

    CN119191387A

  • Surface-doped layered battery positive electrode material as well as preparation method and application thereof

    CN119890292A

  • A surface-doped layered battery cathode material, and a preparation method and application thereof

    CN119890292B

  • Sodium-ion battery and preparation and application of in-situ coating gradient oxygen deficiency positive electrode active material of sodium-ion battery

    CN120033223A

  • O3-phase layered oxide positive electrode material and preparation method and application thereof

    CN121516924A