Microcrystalline graphite negative electrode material and preparation method thereof, lithium ion battery and electric equipment

By using the structure of microcrystalline graphite core, porous carbon cladding layer and surface carbon cladding layer in the microcrystalline graphite negative electrode material, combined with the processes of flotation, drying, crushing, grading, high-temperature purification pore formation and cooling carbon layer deposition, The problem of preparing high-capacity, long-cycle microcrystalline graphite negative electrode materials is solved, and the electrochemical performance and safety performance of the material are significantly improved.

CN118969983APending Publication Date: 2024-11-15SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411010070.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

How to prepare high-capacity, long-circulation microcrystalline graphite negative electrode material to replace scale graphite to meet the performance needs of lithium-ion batteries.

Method used

Using the structure of microcrystalline graphite core, porous carbon cladding layer and surface carbon cladding layer, the porous structure and lithium embedded channel are formed through flotation, drying, crushing, grading, high-temperature purification of pores and cooling carbon layer deposition. microcrystalline graphite negative electrode material.

Benefits of technology

The capacity, rate performance, Coulomb efficiency and cycling performance of microcrystalline graphite anode material is improved, the specific surface area and defects are reduced, and the electrochemical performance and safety performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969983A_ABST
    Figure CN118969983A_ABST
Patent Text Reader

Abstract

The invention provides a microcrystalline graphite negative electrode material and a preparation method thereof, a lithium ion battery and electric equipment, and relates to the technical field of microcrystalline graphite negative electrode materials. The microcrystalline graphite negative electrode material comprises a microcrystalline graphite inner core, a porous carbon coating layer and a surface carbon coating layer, the porous carbon coating layer coats the microcrystalline graphite core; and the surface carbon coating layer coats the porous carbon coating layer. The microcrystalline graphite inner core and the graphitized surface carbon coating layer have more lithium intercalation sites and fewer surface defects, so that the negative electrode material has higher capacity; the porous carbon coating layer has more lithium intercalation channels, so that a guarantee is provided for isotropic lithium intercalation of internal microcrystalline graphite, and the material has more excellent rate capability; the surface carbon coating layer reduces the specific surface area and defects of the material, and the coulombic efficiency and cycle performance of the microcrystalline graphite negative electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of microcrystalline graphite negative electrode materials, and in particular to a microcrystalline graphite negative electrode material and a preparation method thereof, a lithium ion battery and electrical equipment. Background Art

[0002] As the cost of graphitization decreases, the market penetration rate of artificial graphite anodes is gradually increasing. As a new type of anode material, microcrystalline graphite is expected to replace flakes to seize the anode market share due to its low cost and performance advantages brought by its structural characteristics. The preparation of high-capacity, long-cycle microcrystalline graphite anode materials is an important direction for the successful application of microcrystalline graphite anodes.

[0003] Therefore, how to prepare high-capacity and long-cycle microcrystalline graphite negative electrode materials is a problem that needs to be solved urgently. Summary of the invention

[0004] The purpose of this application is to provide a microcrystalline graphite negative electrode material and a preparation method thereof, a lithium ion battery and electrical equipment to solve the above problems.

[0005] To achieve the above objectives, the present application provides a first aspect of a microcrystalline graphite negative electrode material, comprising: a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer;

[0006] The porous carbon coating layer covers the microcrystalline graphite core;

[0007] The surface carbon coating layer covers the porous carbon coating layer.

[0008] Optionally, the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0009] A. The D50 of the microcrystalline graphite core is 7 μm-16 μm;

[0010] B. The tap density of the microcrystalline graphite core is 0.6 g / cc-1.3 g / cc;

[0011] C. the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer include mesophase pitch;

[0012] D. The softening point of the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer is 100° C.-280° C.;

[0013] E. The true density of the microcrystalline graphite negative electrode material is 1.95 g / cc-2.4 g / cc;

[0014] F. The D50 of the microcrystalline graphite negative electrode material is 11 μm-18 μm;

[0015] G. The D90 / D10 of the microcrystalline graphite negative electrode material is 4-7;

[0016] I. The tap density of the microcrystalline graphite negative electrode material is 0.8g / cc-1.3g / cc;

[0017] J. The specific surface area of ​​the microcrystalline graphite negative electrode material is less than 4m 2 / g;

[0018] K. The thickness of the porous carbon coating layer is 30nm-100nm;

[0019] L. The thickness of the surface carbon coating layer is 5nm-20nm;

[0020] M. The carbon content of the microcrystalline graphite negative electrode material is 99.90%-99.99%.

[0021] The second aspect of the present application provides a method for preparing the microcrystalline graphite negative electrode material, comprising:

[0022] The raw ore, the collector and the frother are mixed for flotation to obtain a microcrystalline graphite flotation concentrate;

[0023] The microcrystalline graphite flotation concentrate is dried, crushed and classified to obtain microcrystalline graphite powder;

[0024] Mixing the microcrystalline graphite powder and a carbon source raw material to obtain a microcrystalline graphite precursor;

[0025] Purifying the microcrystalline graphite precursor at high temperature to form pores, thereby obtaining a porous carbon-coated microcrystalline graphite;

[0026] The porous carbon-coated microcrystalline graphite is subjected to cooling carbon layer deposition to obtain a microcrystalline graphite negative electrode material.

[0027] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0028] A. The diameter of the raw ore is 2cm-5cm;

[0029] B. The weight ratio of the raw ore, the collector and the frother is 1000:(5-25):(6-18);

[0030] C. the collector comprises one or more of kerosene, diesel and No. 2 oil;

[0031] D. the foaming agent comprises terpineol;

[0032] E. The grade of the microcrystalline graphite flotation concentrate is 89%-91%;

[0033] F. The flotation includes coarse grinding, fine grinding, scavenging and concentrating.

[0034] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0035] A. the drying comprises flash drying;

[0036] B. The drying air inlet temperature is 200°C-380°C, the mixing temperature is 90°C-130°C, and the air outlet temperature is 40°C-70°C;

[0037] C. The specific surface area of ​​the microcrystalline graphite powder is 5m 2 / g-20m 2 / g.

[0038] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0039] A. The high-temperature purification and pore formation includes one or more of intermittent graphitization, continuous graphitization and high-temperature atmosphere purification;

[0040] B. The temperature of the high-temperature purification and pore making is 1600°C-3450°C, and the time is 8h-24h.

[0041] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0042] A. The temperature of the intermittent graphitization and / or the continuous graphitization is 2800°C-3450°C;

[0043] B. When the Al content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3000° C.-3450° C.;

[0044] C. When the Fe content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3414° C.-3450° C.;

[0045] D. The temperature of the high temperature atmosphere purification is greater than or equal to 1600°C.

[0046] Optionally, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0047] A. The cooling rate before the carbon layer deposition is 60°C-100°C / min;

[0048] B. The constant temperature of the cooling carbon layer deposition is 600°C-800°C, and the constant temperature time is 1h-2h;

[0049] C. The cooling rate after the carbon layer is deposited is 5°C / min-10°C / min.

[0050] A third aspect of the present application provides a lithium-ion battery, comprising the microcrystalline graphite negative electrode material or the microcrystalline graphite negative electrode material prepared by the preparation method of the microcrystalline graphite negative electrode material.

[0051] A fourth aspect of the present application provides an electrical device, including the lithium-ion battery.

[0052] Compared with the prior art, the beneficial effects of this application include:

[0053] The microcrystalline graphite negative electrode material provided in the present application has a microcrystalline graphite core inside and a porous carbon coating layer outside, and the porous carbon coating layer is coated with a surface carbon coating layer on the outer surface. On the first aspect, the microcrystalline graphite core and the graphitized surface carbon coating layer have more lithium insertion sites and fewer surface defects, so that the negative electrode material has a higher capacity; on the second aspect, the porous carbon coating layer has more lithium insertion channels, which provides a guarantee for the isotropic lithium insertion of the internal microcrystalline graphite, and the material has a better rate performance; on the third aspect, the surface carbon coating layer reduces the specific surface area and defects of the material, and the coulombic efficiency and cycle performance of the microcrystalline graphite negative electrode material are improved.

[0054] The preparation method of the microcrystalline graphite negative electrode material provided in the present application utilizes high-temperature purification and pore formation to remove impurities in the microcrystalline graphite powder. While the impurities escape in a gaseous state under high temperature, pores are formed in the coating layer, so that the coating layer has a porous structure, providing more lithium ion migration channels; in the cooling process, the deposition and growth of the carbon layer are controlled by heat preservation, so that the open-pore structure of the microcrystalline graphite in the porous carbon coating layer is converted into a closed-pore structure, effectively reducing the specific surface area of ​​the microcrystalline graphite negative electrode material, and improving the coulombic efficiency, cycle performance and safety performance of the microcrystalline graphite negative electrode material.

[0055] The lithium-ion battery and electrical equipment provided in this application have good coulombic efficiency, cycle performance and safety performance, and excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0057] Figure 1 This is a schematic diagram of the structure of the microcrystalline graphite negative electrode material prepared in Example 3;

[0058] Figure 2 This is a high-magnification SEM image of the microcrystalline graphite negative electrode material prepared in Example 3;

[0059] Figure 3 This is a schematic diagram of the first charge and discharge capacity curve of the microcrystalline graphite negative electrode material prepared in Example 3;

[0060] Figure 4 Schematic diagram of the cycle capacity of the microcrystalline graphite negative electrode material prepared in Example 3. DETAILED DESCRIPTION

[0061] As used herein:

[0062] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0063] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0064] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0065] In these examples, parts and percentages are by mass unless otherwise indicated.

[0066] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0067] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0068] The first aspect of the present application provides a microcrystalline graphite negative electrode material, comprising: a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer;

[0069] The porous carbon coating layer covers the microcrystalline graphite core;

[0070] The surface carbon coating layer covers the porous carbon coating layer.

[0071] In some embodiments, the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0072] A. The D50 of the microcrystalline graphite core is 7 μm-16 μm;

[0073] Optionally, the D50 of the microcrystalline graphite core may be 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm or any value between 7 μm and 16 μm;

[0074] B. The tap density of the microcrystalline graphite core is 0.6 g / cc-1.3 g / cc;

[0075] Optionally, the tap density of the microcrystalline graphite core may be 0.6 g / cc, 0.8 g / cc, 1.0 g / cc, 1.2 g / cc, 1.3 g / cc, or any value between 0.6 g / cc and 1.3 g / cc;

[0076] C. the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer include mesophase pitch;

[0077] Optionally, the mesophase pitch includes petroleum pitch and / or coal pitch.

[0078] D. The softening point of the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer is 100° C.-280° C.;

[0079] Optionally, the softening point of the carbon source raw material of the porous carbon coating layer and the surface carbon coating layer can be 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C or any value between 100°C and 280°C;

[0080] E. The true density of the microcrystalline graphite negative electrode material is 1.95 g / cc-2.4 g / cc;

[0081] Optionally, the true density of the microcrystalline graphite negative electrode material can be 1.95 g / cc, 2.00 g / cc, 2.05 g / cc, 2.10 g / cc, 2.15 g / cc, 2.20 g / cc, 2.25 g / cc, 2.30 g / cc, 2.35 g / cc, 2.40 g / cc or any value between 1.95 g / cc and 2.4 g / cc;

[0082] F. The D50 of the microcrystalline graphite negative electrode material is 11 μm-18 μm;

[0083] Optionally, the D50 of the microcrystalline graphite negative electrode material may be 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm or any value between 11 μm and 18 μm;

[0084] G. The D90 / D10 of the microcrystalline graphite negative electrode material is 4-7;

[0085] Optionally, the D90 / D10 of the microcrystalline graphite negative electrode material may be 4, 5, 6, 7 or any value between 4 and 7;

[0086] I. The tap density of the microcrystalline graphite negative electrode material is 0.8g / cc-1.3g / cc;

[0087] Optionally, the tap density of the microcrystalline graphite negative electrode material may be 0.8 g / cc, 0.9 g / cc, 1.0 g / cc, 1.1 g / cc, 1.2 g / cc, 1.3 g / cc or any value between 0.8 g / cc and 1.3 g / cc;

[0088] J. The specific surface area of ​​the microcrystalline graphite negative electrode material is less than 4m 2 / g;

[0089] Optionally, the specific surface area of ​​the microcrystalline graphite negative electrode material can be 0.1 m 2 / g, 1m 2 / g, 2m 2 / g, 3m 2 / g or <4m 2 Any value of / g;

[0090] K. The thickness of the porous carbon coating layer is 30nm-100nm;

[0091] Optionally, the thickness of the porous carbon coating layer may be 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm or any value between 30 nm and 100 nm;

[0092] L. The thickness of the surface carbon coating layer is 5nm-20nm;

[0093] Optionally, the thickness of the surface carbon coating layer may be 5 nm, 10 nm, 15 nm, 20 nm or any value between 5 nm and 20 nm;

[0094] M. The carbon content of the microcrystalline graphite negative electrode material is 99.90%-99.99%.

[0095] Optionally, the carbon content of the microcrystalline graphite negative electrode material can be 99.90%, 99.91%, 99.92%, 99.93%, 99.94%, 99.95%, 99.96%, 99.97%, 99.98%, 99.99% or any value between 99.90% and 99.99%.

[0096] The second aspect of the present application provides a method for preparing the microcrystalline graphite negative electrode material, comprising:

[0097] The raw ore, the collector and the frother are mixed for flotation to obtain a microcrystalline graphite flotation concentrate;

[0098] The microcrystalline graphite flotation concentrate is dried, crushed and classified to obtain microcrystalline graphite powder;

[0099] Mixing the microcrystalline graphite powder and a carbon source raw material to obtain a microcrystalline graphite precursor;

[0100] Purifying the microcrystalline graphite precursor at high temperature to form pores, thereby obtaining a porous carbon-coated microcrystalline graphite;

[0101] The porous carbon-coated microcrystalline graphite is subjected to cooling carbon layer deposition to obtain a microcrystalline graphite negative electrode material.

[0102] It should be noted that the impurity content of the original ore is relatively high (the carbon content is generally 60-80%). Direct high-temperature purification and pore making without flotation will lead to uneven impurity escape, excessively large specific surface area of ​​the microcrystalline graphite negative electrode material, and a series of defects such as low vibration and true density. In addition, excessive impurity content can easily cause corrosion and blockage to high-temperature purification equipment.

[0103] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0104] A. The diameter of the raw ore is 2cm-5cm;

[0105] Optionally, the diameter of the raw ore can be 2 cm, 3 cm, 4 cm, 5 cm or any value between 2 cm and 5 cm;

[0106] B. The weight ratio of the raw ore, the collector and the frother is 1000:(5-25):(6-18);

[0107] Optionally, the weight ratio of the raw ore to the collector can be 1000:5, 1000:10, 1000:15, 1000:20, 1000:25 or any value between 1000:(5-25), and the weight ratio of the raw ore to the frother can be 1000:6, 1000:8, 1000:10, 1000:12, 1000:14, 1000:16, 1000:18 or any value between 1000:(6-18);

[0108] C. the collector comprises one or more of kerosene, diesel and No. 2 oil;

[0109] D. the foaming agent comprises terpineol;

[0110] E. The grade of the microcrystalline graphite flotation concentrate is 89%-91%;

[0111] Optionally, the grade of the microcrystalline graphite flotation concentrate may be 89%, 90%, 91% or any value between 89% and 91%;

[0112] It should be noted that when the grade of microcrystalline graphite flotation concentrate is 89%-91% and the total impurity content is 9%-11%, the impurities can be controlled to escape uniformly after high-temperature purification, and the pore structure of the microcrystalline graphite coating layer is uniform. The types of impurities in microcrystalline graphite mainly include silicates, aluminosilicates, quartz, carbonates, metal oxides, etc. (generally more silicon oxide and aluminum oxide).

[0113] F. The flotation includes coarse grinding, fine grinding, scavenging and concentrating.

[0114] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0115] A. the drying comprises flash drying;

[0116] It should be noted that flash drying has high efficiency and the drying temperature will not affect the graphite surface and internal impurities. Of course, any drying method such as an oven or tunnel kiln with a temperature in the insulation section not exceeding 200°C can achieve the technical effect achieved in this application.

[0117] B. The drying air inlet temperature is 200°C-380°C, the mixing temperature is 90°C-130°C, and the air outlet temperature is 40°C-70°C;

[0118] Optionally, the drying air inlet temperature may be 200°C, 250°C, 300°C, 350°C, 380°C or any value between 200°C and 380°C, the mixing temperature may be 90°C, 100°C, 110°C, 120°C, 130°C or any value between 90°C and 130°C, and the air outlet temperature may be 40°C, 50°C, 60°C, 70°C or any value between 40°C and 70°C;

[0119] It should be noted that the mixing temperature is the temperature between the inlet and outlet air during drying.

[0120] C. The specific surface area of ​​the microcrystalline graphite powder is 5m 2 / g-20m 2 / g.

[0121] Optionally, the specific surface area of ​​the microcrystalline graphite powder can be 5m 2 / g, 10m 2 / g, 15m 2 / g, 20m 2 / g or 5m 2 / g-20m 2 Any value between / g.

[0122] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0123] A. The high-temperature purification and pore formation includes one or more of intermittent graphitization, continuous graphitization and high-temperature atmosphere purification;

[0124] It should be noted that, in intermittent graphitization, continuous graphitization and high-temperature atmosphere purification, intermittent graphitization is to put microcrystalline graphite into a container, and by heating to a certain temperature and keeping it warm for a period of time, the impurities of the microcrystalline graphite in the container escape (beneficial effect: stable temperature control, more thorough impurity escape), generally, Chisun furnace, series furnace, vacuum graphitization furnace, box furnace and other high-temperature graphitization devices are used for batch loading of materials; continuous graphitization is to use a continuous feeding method to remove impurities and form pores in the high-temperature section of the equipment by granulation or direct feeding (beneficial effect: high production efficiency and lower energy consumption); high-temperature atmosphere purification is to add a certain amount of reducing agent to graphite, roast it at a certain temperature and a specific atmosphere, and then introduce chlorine gas for chemical reaction, so that the valuable metals in the material are converted into chlorides and complexes with lower melting and boiling points in the gas phase or condensed phase and escape, thereby separating from the other components to achieve the purpose of purification and pore formation (beneficial effect: lowest energy consumption).

[0125] B. The temperature of the high-temperature purification and pore making is 1600°C-3450°C, and the time is 8h-24h.

[0126] Optionally, the temperature of high-temperature purification and pore making can be 1600℃, 2000℃, 2500℃, 3000℃, 3450℃ or any value between 1600℃-3450℃, and the time can be 8h, 10h, 15h, 20h, 24h or any value between 8h-24h.

[0127] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0128] A. The temperature of the intermittent graphitization and / or the continuous graphitization is 2800°C-3450°C;

[0129] Optionally, the temperature of intermittent graphitization and / or continuous graphitization may be 2800°C, 2900°C, 3000°C, 3100°C, 3200°C, 3300°C, 3400°C or any value between 2800°C and 3450°C;

[0130] It should be noted that the boiling point of the impure metal oxides in microcrystalline graphite is generally above 2800°C, among which the boiling point of iron oxide is as high as 3414°C. The reaction temperature of intermittent graphitization and / or continuous graphitization is set based on the boiling point of the impurity metal oxides.

[0131] B. When the Al content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3000° C.-3450° C.;

[0132] Optionally, when the Al content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3000°C, 3050°C, 3100°C, 3150°C, 3200°C, 3250°C, 3300°C, 3350°C, 3400°C, 3450°C or any value between 3000°C and 3450°C;

[0133] It should be noted that the boiling point of aluminum oxide is 2980° C. When the Al content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization needs to be greater than 3000° C. to effectively release aluminum.

[0134] C. When the Fe content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3414-3450° C.;

[0135] Optionally, when the Fe content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization may be 3414°C, 3415°C, 3420°C, 3425°C, 3430°C, 3440°C, 3450°C or any value between 3414°C and 3450°C;

[0136] It should be noted that when the Fe content in the microcrystalline graphite precursor is greater than 5000 ppm, the boiling point of iron oxide is 3414° C., and the temperature of the intermittent graphitization and / or the continuous graphitization needs to be greater than 3414° C. to effectively release iron.

[0137] D. The temperature of the high temperature atmosphere purification is greater than or equal to 1600°C.

[0138] Optionally, the temperature of the high temperature atmosphere purification may be 1600°C, 2000°C, 2500°C, 3000°C, 3450°C or any value between 1600°C and 3450°C.

[0139] In some embodiments, the method for preparing the microcrystalline graphite negative electrode material satisfies at least one of the following conditions:

[0140] A. The cooling rate before the carbon layer deposition is 60°C-100°C / min;

[0141] Optionally, the cooling rate before the carbon layer deposition can be 60°C, 70°C, 80°C, 90°C, 100°C or any value between 60°C and 100°C / min;

[0142] B. The constant temperature of the cooling carbon layer deposition is 600°C-800°C, and the constant temperature time is 1h-2h;

[0143] Optionally, the constant temperature of the cooling carbon layer deposition can be 600°C, 650°C, 700°C, 750°C, 800°C or any value between 600°C and 800°C, and the constant temperature time can be 1h, 1.5h, 2h or any value between 1h and 2h;

[0144] C. The cooling rate after the carbon layer is deposited is 5°C / min-10°C / min.

[0145] Optionally, the cooling rate after the carbon layer is deposited can be 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or any value between 5°C / min and 10°C / min.

[0146] It should be noted that controlling the carbon layer deposition temperature at 600-800℃ is beneficial to the formation of the outermost carbon layer skeleton, avoiding the carbon layer particles being too large and the porosity being too high which affects the initial coulombic efficiency of the negative electrode material. Controlling the cooling rate at 5℃-10℃ further controls the integrity of the outer carbon layer and the uniformity of its thickness.

[0147] A third aspect of the present application provides a lithium-ion battery, comprising the microcrystalline graphite negative electrode material or the microcrystalline graphite negative electrode material prepared by the preparation method of the microcrystalline graphite negative electrode material.

[0148] A fourth aspect of the present application provides an electrical device, including the lithium-ion battery.

[0149] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0150] Example 1

[0151] This embodiment provides a microcrystalline graphite negative electrode material, comprising a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer, wherein the porous carbon coating layer coats the microcrystalline graphite core, and the surface carbon coating layer coats the porous carbon coating layer;

[0152] Among them, the D50 of the microcrystalline graphite core is 8.5μm, and the tap density is 0.653g / cc; the carbon source raw material of the porous carbon coating layer and the surface carbon coating layer is petroleum asphalt; the true density of the microcrystalline graphite negative electrode material is 2.04g / cc, the D50 of the microcrystalline graphite negative electrode material is 11.3μm, D90 / D10 is 4.4, the tap density is 0.898g / cc, and the specific surface area is 3.0m 2 / g, the thickness of the porous carbon coating layer is 68nm, the thickness of the surface carbon coating layer is 18nm, and the carbon content of the microcrystalline graphite negative electrode material is 99.99%.

[0153] This embodiment also provides a method for preparing a microcrystalline graphite negative electrode material, comprising:

[0154] S1. Crushing: By crushing the raw ore, microcrystalline graphite raw ore particles with a diameter of 2cm-5cm are obtained;

[0155] S2, flotation: add 5 parts of collector kerosene and 6 parts of foaming agent pine alcohol to 1000 parts of microcrystalline graphite ore particles, and obtain microcrystalline graphite flotation concentrate through coarse grinding, fine grinding, scavenging and selection. The grade of the microcrystalline graphite flotation concentrate is 90.3%;

[0156] S3, drying: the microcrystalline graphite flotation concentrate is flash dried, the inlet air temperature of the flash drying is 350°C, the mixing temperature is 124°C, and the outlet air temperature is 66°C, to obtain a dry microcrystalline graphite flotation concentrate;

[0157] S4. Crushing and Classification: The dried product of microcrystalline graphite flotation concentrate is further crushed and classified. The specific surface area of ​​microcrystalline graphite powder is 10.34m 2 / g;

[0158] S5, coating and mixing: adding 15% of petroleum asphalt, a carbon source raw material, to the microcrystalline graphite powder, and mixing them evenly to obtain a microcrystalline graphite precursor, wherein the Al content in the microcrystalline graphite precursor is 5686ppm, and the Fe content is 5797ppm;

[0159] S6, purification and pore formation: the microcrystalline graphite precursor is subjected to high-temperature purification and pore formation by intermittent graphitization at a temperature of 3450°C for 12 hours to obtain a porous carbon-coated microcrystalline graphite;

[0160] S7, carbon layer deposition: after high-temperature purification and pore formation, pre-cooling begins, with a pre-cooling rate of 100°C / min. After pre-cooling to 600°C, the constant temperature stage is entered, and the constant temperature stage lasts for 2 hours. After the constant temperature stage, the temperature is continued to be lowered to room temperature, and the cooling rate after constant temperature is 10°C / min to obtain microcrystalline graphite negative electrode material.

[0161] The electrochemical performance of the microcrystalline graphite negative electrode material was tested, and the initial charge and discharge specific capacity was 364mAh / g, the initial coulombic efficiency was 94.1%, the capacity retention rate after 600 cycles at 1C current was 96.1%, the 3C lithium removal capacity retention rate was 98.7%, and the 3C lithium insertion capacity retention rate was 91.2%.

[0162] Example 2

[0163] This embodiment provides a microcrystalline graphite negative electrode material, comprising a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer, wherein the porous carbon coating layer coats the microcrystalline graphite core, and the surface carbon coating layer coats the porous carbon coating layer;

[0164] Among them, the D50 of the microcrystalline graphite core is 15.6μm, and the tap density is 0.772g / cc; the carbon source raw material of the porous carbon coating layer and the surface carbon coating layer is coal tar; the true density of the microcrystalline graphite negative electrode material is 2.08g / cc, the D50 of the microcrystalline graphite negative electrode material is 17.3μm, D90 / D10 is 6.2, the tap density is 1.132g / cc, and the specific surface area is 3.2m 2 / g, the thickness of the porous carbon coating layer is 40nm, the thickness of the surface carbon coating layer is 10nm, and the carbon content of the microcrystalline graphite negative electrode material is 99.99%.

[0165] This embodiment also provides a method for preparing a microcrystalline graphite negative electrode material, comprising:

[0166] S1. Crushing: By crushing the raw ore, microcrystalline graphite raw ore particles with a diameter of 2cm-5cm are obtained;

[0167] S2, flotation: add 10 parts of collector kerosene and 11 parts of foaming agent pine alcohol to 1000 parts of microcrystalline graphite ore particles, and obtain microcrystalline graphite flotation concentrate through coarse grinding, fine grinding, scavenging and selection. The grade of the microcrystalline graphite flotation concentrate is 90.5%;

[0168] S3, drying: the microcrystalline graphite flotation concentrate is flash dried, the inlet air temperature of the flash drying is 300°C, the mixing temperature is 110°C, and the outlet air temperature is 57°C, to obtain a dry microcrystalline graphite flotation concentrate;

[0169] S4. Crushing and Classification: The dried product of microcrystalline graphite flotation concentrate is further crushed and classified. The specific surface area of ​​microcrystalline graphite powder is 13.4m 2 / g;

[0170] S5, coating and mixing: adding 8% of coal tar pitch, a carbon source raw material, to the microcrystalline graphite powder, and mixing them evenly to obtain a microcrystalline graphite precursor, wherein the Al content in the microcrystalline graphite precursor is 10012ppm, and the Fe content is 4576ppm;

[0171] S6, purification and pore formation: the microcrystalline graphite precursor is purified and pore-formed by continuous graphitization at high temperature, the temperature is 3200°C, the time is 18h, and a porous carbon-coated microcrystalline graphite is obtained;

[0172] S7, carbon layer deposition: after high-temperature purification and pore formation, pre-cooling begins, with a pre-cooling rate of 100°C / min. After pre-cooling to 600°C, the system enters a constant temperature stage for 2 hours. After the constant temperature stage, the system continues to cool to room temperature, with a cooling rate of 8°C / min to obtain a microcrystalline graphite negative electrode material.

[0173] The electrochemical performance of the microcrystalline graphite negative electrode material was tested, and the initial charge and discharge specific capacity was 367mAh / g, the initial coulombic efficiency was 94.4%, the capacity retention rate after 600 cycles at 1C current was 96.5%, the 3C lithium removal capacity retention rate was 98.4%, and the 3C lithium insertion capacity retention rate was 89.1%.

[0174] Example 3

[0175] This embodiment provides a microcrystalline graphite negative electrode material, comprising a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer, wherein the porous carbon coating layer coats the microcrystalline graphite core, and the surface carbon coating layer coats the porous carbon coating layer;

[0176] Among them, the D50 of the microcrystalline graphite core is 14.3μm, and the tap density is 0.854g / cc; the carbon source raw material of the porous carbon coating layer and the surface carbon coating layer is coal tar; the true density of the microcrystalline graphite negative electrode material is 2.33g / cc, the D50 of the microcrystalline graphite negative electrode material is 16.1μm, D90 / D10 is 4.5, the tap density is 1.192g / cc, and the specific surface area is 2.1m 2 / g, the thickness of the porous carbon coating layer is 38nm, the thickness of the surface carbon coating layer is 8nm, and the carbon content of the microcrystalline graphite negative electrode material is 99.98%.

[0177] This embodiment also provides a method for preparing a microcrystalline graphite negative electrode material, comprising:

[0178] S1. Crushing: By crushing the raw ore, microcrystalline graphite raw ore particles with a diameter of 2cm-5cm are obtained;

[0179] S2, flotation: add 15 parts of collector kerosene and 18 parts of foaming agent pine alcohol to 1000 parts of microcrystalline graphite ore particles, and obtain microcrystalline graphite flotation concentrate through coarse grinding, fine grinding, scavenging and selection. The grade of the microcrystalline graphite flotation concentrate is 89.7%;

[0180] S3, drying: the microcrystalline graphite flotation concentrate is flash dried, the inlet air temperature of the flash drying is 220°C, the mixing temperature is 98°C, and the outlet air temperature is 42°C, to obtain a dry microcrystalline graphite flotation concentrate;

[0181] S4. Crushing and Classification: The dried product of microcrystalline graphite flotation concentrate is further crushed and classified. The specific surface area of ​​microcrystalline graphite powder is 10.2m 2 / g;

[0182] S5, coating and mixing: adding 5% of coal tar pitch, a carbon source raw material, to the microcrystalline graphite powder, and mixing them evenly to obtain a microcrystalline graphite precursor, wherein the Al content in the microcrystalline graphite precursor is 4679ppm, and the Fe content is 4220ppm;

[0183] S6, purification and pore formation: the microcrystalline graphite precursor is purified and pore-formed at high temperature by continuous graphitization at a temperature of 2900°C for 24 hours to obtain a porous carbon-coated microcrystalline graphite;

[0184] S7, carbon layer deposition: after high-temperature purification and pore formation, pre-cooling begins, with a pre-cooling rate of 80°C / min. After pre-cooling to 600°C, the constant temperature stage is entered, and the constant temperature stage lasts for 2 hours. After the constant temperature stage, the temperature is continued to be lowered to room temperature, and the cooling rate after constant temperature is 5°C / min to obtain microcrystalline graphite negative electrode material.

[0185] The structure of the microcrystalline graphite negative electrode material is as follows Figure 1As shown, it can be seen that the core of the microcrystalline graphite negative electrode material is microcrystalline graphite filled with gaps, and the outer layer is a porous carbon coating layer and a surface carbon coating layer. The microcrystalline graphite negative electrode material has sufficient lithium insertion sites, and the porous carbon coating layer provides more lithium insertion channels to ensure the isotropic lithium insertion of the internal microcrystalline graphite. The microcrystalline graphite negative electrode material has more excellent rate performance.

[0186] The high-magnification SEM image of the microcrystalline graphite negative electrode material is as follows Figure 2 As shown, the porous carbon coating layer is covered with a complete surface carbon coating layer, and the open-pore structure of the porous carbon coating layer is transformed into a closed-pore structure during the cooling stage, which effectively reduces the specific surface area of ​​the negative electrode material and improves the coulombic efficiency, cycle performance and safety performance of the material.

[0187] The electrochemical performance of the microcrystalline graphite negative electrode material was tested, and the initial charge and discharge specific capacity was as follows Figure 3 As shown, it is 365mAh / g, the first coulombic efficiency is 94.5%, and the 600-cycle capacity at 1C current is as follows Figure 4 As shown, the retention rate is 97.3%, the 3C lithium desorption capacity retention rate is 97.2%, and the 3C lithium insertion capacity retention rate is 88.4%.

[0188] Example 4

[0189] This embodiment provides a microcrystalline graphite negative electrode material, comprising a microcrystalline graphite core, a porous carbon coating layer and a surface carbon coating layer, wherein the porous carbon coating layer coats the microcrystalline graphite core, and the surface carbon coating layer coats the porous carbon coating layer;

[0190] Among them, the D50 of the microcrystalline graphite core is 15.1μm, and the tap density is 0.972g / cc; the carbon source raw material of the porous carbon coating layer and the surface carbon coating layer is the intermediate phase asphalt naphthalene asphalt; the true density of the microcrystalline graphite negative electrode material is 2.28g / cc, the D50 of the microcrystalline graphite negative electrode material is 17.6μm, D90 / D10 is 4.1, the tap density is 1.216g / cc, and the specific surface area is 2.1m 2 / g, the thickness of the porous carbon coating layer is 55μm, the thickness of the surface carbon coating layer is 12μm, and the carbon content of the microcrystalline graphite negative electrode material is 99.95%.

[0191] This embodiment also provides a method for preparing a microcrystalline graphite negative electrode material, comprising:

[0192] S1. Crushing: By crushing the raw ore, microcrystalline graphite raw ore particles with a diameter of 2cm-5cm are obtained;

[0193] S2, flotation: add 25 parts of collector kerosene and 12 parts of foaming agent pine alcohol to 1000 parts of microcrystalline graphite ore particles, and obtain microcrystalline graphite flotation concentrate through coarse grinding, fine grinding, scavenging and selection. The grade of the microcrystalline graphite flotation concentrate is 90.7%;

[0194] S3, drying: the microcrystalline graphite flotation concentrate is flash dried, the inlet air temperature of the flash drying is 374°C, the mixing temperature is 104°C, and the outlet air temperature is 48°C, to obtain a dry microcrystalline graphite flotation concentrate;

[0195] S4. Crushing and Classification: The dried product of microcrystalline graphite flotation concentrate is further crushed and classified. The specific surface area of ​​microcrystalline graphite powder is 12.1m 2 / g;

[0196] S5, coating and mixing: adding 10% of the carbon source raw material mesophase asphalt naphthalene asphalt to the microcrystalline graphite powder, mixing evenly, to obtain a microcrystalline graphite precursor, wherein the Al content in the microcrystalline graphite precursor is 7948ppm, and the Fe content is 8796ppm;

[0197] S6, purification and pore formation: the microcrystalline graphite precursor is purified by high temperature atmosphere (chlorine) purification at high temperature, the temperature is 1700°C, the time is 15h, and the porous carbon coating layer of microcrystalline graphite is obtained;

[0198] S7, carbon layer deposition: after high-temperature purification and pore formation, pre-cooling begins, with a pre-cooling rate of 60°C / min. After pre-cooling to 600°C, the constant temperature stage is entered, and the constant temperature stage lasts for 1.5 hours. After the constant temperature stage, the temperature is continued to be lowered to room temperature, and the cooling rate after constant temperature is 8°C / min to obtain microcrystalline graphite negative electrode material.

[0199] The electrochemical performance of the microcrystalline graphite negative electrode material was tested, and the initial charge and discharge specific capacity was 359 mAh / g, the initial coulombic efficiency was 94.5%, the capacity retention rate after 600 cycles at 1C current was 97.0%, the 3C lithium removal capacity retention rate was 96.8%, and the 3C lithium insertion capacity retention rate was 88.2%.

[0200] Comparative Example 1

[0201] This comparative example provides a graphite negative electrode material and a preparation method thereof, which is different from Example 4 in that the temperature of the high-temperature atmosphere purification method in this comparative example is 1550°C, and other conditions are consistent with Example 4.

[0202] The graphite negative electrode material prepared by the above-mentioned preparation method of graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 363 mAh / g, the initial coulombic efficiency was 92.7%, the capacity retention rate of 600 cycles at 1C current was 93.0%, the 3C lithium removal capacity retention rate was 93.5%, and the 3C lithium insertion capacity retention rate was 81.7%.

[0203] Comparative Example 2

[0204] This comparative example provides a graphite negative electrode material and a preparation method thereof, which is different from Example 3 in that the temperature of high-temperature purification and pore formation in this comparative example is 2700°C, and other conditions are consistent with Example 1.

[0205] The graphite negative electrode material prepared by the above-mentioned preparation method of graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 360 mAh / g, the initial coulombic efficiency was 92.5%, the capacity retention rate of 600 cycles at 1C current was 93.7%, the 3C lithium removal capacity retention rate was 90.4%, and the 3C lithium insertion capacity retention rate was 78.9%.

[0206] Comparative Example 3

[0207] This comparative example provides a graphite negative electrode material and a preparation method thereof, which differs from Example 1 in that the Fe content prepared in step S5 of this comparative example is greater than 5000 ppm, and high-temperature purification and pore formation are carried out by continuous graphitization at a temperature of 3000°C, and other conditions are consistent with Example 1.

[0208] The graphite negative electrode material prepared by the above-mentioned preparation method of graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 365 mAh / g, the initial coulombic efficiency was 88.2%, the capacity retention rate of 600 cycles at 1C current was 90.7%, the 3C lithium removal capacity retention rate was 87.6%, and the 3C lithium insertion capacity retention rate was 75.2%.

[0209] Comparative Example 4

[0210] This comparative example provides a graphite negative electrode material and a preparation method thereof, which differs from Example 2 in that the Al content prepared in step S5 of this comparative example is greater than 5000 ppm, and high-temperature purification and pore formation are performed by continuous graphitization at a temperature of 2900°C. Other conditions are consistent with Example 2.

[0211] The graphite negative electrode material prepared by the above-mentioned preparation method of graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 359 mAh / g, the initial coulombic efficiency was 91.7%, the capacity retention rate of 600 cycles at 1C current was 91.2%, the 3C lithium removal capacity retention rate was 88.2%, and the 3C lithium insertion capacity retention rate was 77.4%.

[0212] Comparative Example 5

[0213] This comparative example provides a graphite negative electrode material and a preparation method thereof, which is different from Example 1 in that the cooling rate before the carbon layer deposition in this comparative example is 50°C / min, the constant temperature insulation time is 0.5h, and other conditions are consistent with Example 1.

[0214] The graphite negative electrode material prepared by the above-mentioned preparation method of graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 363.2 mAh / g, the initial coulombic efficiency was 92.2%, the capacity retention rate of 600 cycles at 1C current was 92.4%, the 3C lithium removal capacity retention rate was 93.5%, and the 3C lithium insertion capacity retention rate was 81.6%.

[0215] Comparative Example 6

[0216] This comparative example provides a microcrystalline graphite negative electrode material, which differs from Example 1 in that an S6 process is added before the S5 process, the microcrystalline graphite is first purified to obtain high-purity microcrystalline graphite with a carbon content of 99.99%, and then the mixture is coated and purified at high temperature. This comparative example does not provide a porous carbon coating layer, and the rest is consistent with Example 1.

[0217] The above graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 365.3 mAh / g, the initial coulombic efficiency was 94.0%, the capacity retention rate after 600 cycles at 1C current was 96.4%, the capacity retention rate after 3C lithium removal was 89.9%, and the capacity retention rate after 3C lithium insertion was 78.4%.

[0218] Comparative Example 7

[0219] This comparative example provides a microcrystalline graphite negative electrode material, which is different from Example 1 in that this comparative example does not have an S7 process (no surface carbon coating layer is provided, and the rest is consistent with Example 1).

[0220] The above graphite negative electrode material was subjected to electrochemical testing, and the initial charge and discharge specific capacity was 364.8 mAh / g, the initial coulombic efficiency was 88.2%, the capacity retention rate after 600 cycles at 1C current was 90.0%, the capacity retention rate after 3C lithium removal was 91.4%, and the capacity retention rate after 3C lithium insertion was 80.8%.

[0221] The results of the embodiments and comparative examples obtained above were tested, including specific surface area test, carbon content test, tap density test, particle size test and true density test method. The specific test results are shown in Table 1.

[0222] Table 1 Performance test

[0223]

[0224] From the above experimental results, it can be seen that according to the parameters described in the scheme of the present invention, the microcrystalline graphite negative electrode material with a carbon content of ≥99.9% can be controlled to have excellent electrochemical properties, significantly reduced impurity content, and a specific surface area of ​​4m 2 / g or less, the first efficiency and cycle performance of the negative electrode material are improved, and the rate performance is better.

[0225] In comparative example 1, the temperature was too low during the atmosphere purification process, resulting in poor purification effect. The carbon content of the finished product was only 99.45%. The incomplete removal of impurities led to increased side reactions of the materials, and the first effect and cycle stability deteriorated.

[0226] In Comparative Example 2, the contents of Al and Fe are both less than 5000 ppm, but the intermittent graphitization temperature is only 2700° C., resulting in that the aluminum oxide and iron oxide impurities in the microcrystalline graphite cannot be completely removed, and the carbon content of the finished product is low.

[0227] In Comparative Example 3, the impurity Fe content is high, and the purification temperature at 3000° C. cannot completely remove the iron oxide in the microcrystalline graphite, which also leads to a low carbon content.

[0228] In Comparative Example 4, due to the high content of Al element impurities, the purification temperature at 2900° C. cannot completely remove the aluminum oxide impurities in the microcrystalline graphite, and the carbon content is relatively low.

[0229] In comparative example 5, the cooling rate during the carbon layer deposition process is too fast, resulting in uneven carbon layer deposition. The outermost carbon coating layer cannot completely cover the internal honeycomb structure. The final product has a too large surface area, increased side reactions, reduced initial efficiency, deteriorated cycle performance, and poor rate performance.

[0230] Comparative Example 6 does not have a pore-forming process. After the impurities in the microcrystalline graphite are completely removed, asphalt is added for high-temperature graphitization, resulting in a reduction in the pore structure of the outer coating layer of the microcrystalline graphite core, a reduction in lithium ion transmission channels, and poor rate performance.

[0231] In comparative example 7, there is no carbon layer deposition process, and the outermost layer is a honeycomb carbon layer structure, which leads to a larger material specific surface area, increased side reactions, reduced first efficiency, deteriorated cycle performance, and poor rate performance.

[0232] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0233] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A microcrystalline graphite negative electrode material, characterized in that: include: Microcrystalline graphite core, porous carbon coating layer and surface carbon coating layer; The porous carbon coating layer covers the microcrystalline graphite core; The surface carbon coating layer covers the porous carbon coating layer.

2. The microcrystalline graphite negative electrode material according to claim 1, characterized in that: At least one of the following conditions is met: A. The D50 of the microcrystalline graphite core is 7 μm-16 μm; B. The tap density of the microcrystalline graphite core is 0.6 g / cc-1.3 g / cc; C. the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer include mesophase pitch; D. The softening point of the carbon source raw materials of the porous carbon coating layer and the surface carbon coating layer is 100° C.-280° C.; E. The true density of the microcrystalline graphite negative electrode material is 1.95 g / cc-2.4 g / cc; F. The D50 of the microcrystalline graphite negative electrode material is 11 μm-18 μm; G. The D90 / D10 of the microcrystalline graphite negative electrode material is 4-7; I. The tap density of the microcrystalline graphite negative electrode material is 0.8g / cc-1.3g / cc; J. The specific surface area of ​​the microcrystalline graphite negative electrode material is less than 4m 2 / g; K. The thickness of the porous carbon coating layer is 30nm-100nm; L. The thickness of the surface carbon coating layer is 5nm-20nm; M. The carbon content of the microcrystalline graphite negative electrode material is 99.90%-99.99%.

3. A method for preparing the microcrystalline graphite negative electrode material according to claim 1 or 2, characterized in that: include: The raw ore, the collector and the frother are mixed for flotation to obtain a microcrystalline graphite flotation concentrate; The microcrystalline graphite flotation concentrate is dried, crushed and classified to obtain microcrystalline graphite powder; Mixing the microcrystalline graphite powder and a carbon source raw material to obtain a microcrystalline graphite precursor; Purifying the microcrystalline graphite precursor at high temperature to form pores, thereby obtaining a porous carbon-coated microcrystalline graphite; The porous carbon-coated microcrystalline graphite is subjected to cooling carbon layer deposition to obtain a microcrystalline graphite negative electrode material.

4. The method for preparing the microcrystalline graphite negative electrode material according to claim 3, characterized in that: At least one of the following conditions is met: A. The diameter of the raw ore is 2cm-5cm; B. The weight ratio of the raw ore, the collector and the frother is 1000:(5-25):(6-18); C. the collector comprises one or more of kerosene, diesel and No. 2 oil; D. the foaming agent comprises terpineol; E. The grade of the microcrystalline graphite flotation concentrate is 89%-91%; F. The flotation includes coarse grinding, fine grinding, scavenging and concentrating.

5. The method for preparing the microcrystalline graphite negative electrode material according to claim 3, characterized in that: At least one of the following conditions is met: A. the drying comprises flash drying; B. The drying air inlet temperature is 200°C-380°C, the mixing temperature is 90°C-130°C, and the air outlet temperature is 40°C-70°C; C. The specific surface area of ​​the microcrystalline graphite powder is 5m 2 / g-20m 2 / g.

6. The method for preparing the microcrystalline graphite negative electrode material according to claim 3, characterized in that: At least one of the following conditions is met: A. The high-temperature purification and pore formation includes one or more of intermittent graphitization, continuous graphitization and high-temperature atmosphere purification; B. The temperature of the high-temperature purification and pore making is 1600°C-3450°C, and the time is 8h-24h.

7. The method for preparing the microcrystalline graphite negative electrode material according to claim 6, characterized in that: At least one of the following conditions is met: A. The temperature of the intermittent graphitization and / or the continuous graphitization is 2800°C-3450°C; B. When the Al content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3000° C.-3450° C.; C. When the Fe content in the microcrystalline graphite precursor is greater than 5000 ppm, the temperature of the intermittent graphitization and / or the continuous graphitization is 3414° C.-3450° C.; D. The temperature of the high temperature atmosphere purification is greater than or equal to 1600°C.

8. The method for preparing the microcrystalline graphite negative electrode material according to any one of claims 3 to 7, characterized in that: At least one of the following conditions is met: A. The cooling rate before the carbon layer deposition is 60°C-100°C / min; B. The constant temperature of the cooling carbon layer deposition is 600°C-800°C, and the constant temperature time is 1h-2h; C. The cooling rate after the carbon layer is deposited is 5°C / min-10°C / min.

9. A lithium ion battery, characterized in that: The invention relates to a microcrystalline graphite negative electrode material prepared by the microcrystalline graphite negative electrode material according to claim 1 or 2 or the microcrystalline graphite negative electrode material prepared by the preparation method of the microcrystalline graphite negative electrode material according to any one of claims 3 to 8.

10. An electrical equipment, characterized in that: Includes the lithium ion battery as claimed in claim 9.

Citation Information

Cited By

  • Negative electrode material and preparation method and application thereof

    CN120727789A

  • Ultrahigh-capacity spherical graphite negative electrode material and production method thereof

    CN120933329A